A masonry adhesive and its preparation method and application, masonry mortar and its separation method
By using quicklime, gypsum powder, fly ash, carbonized garden waste, and propylene glycol block polyether to create a masonry adhesive, the problem of traditional cement mortar being difficult to separate is solved, achieving high strength and easy separation of masonry mortar, and reducing resource waste and costs.
Patent Information
- Application Number
- CN202211558307.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2042-12-06
AI Technical Summary
Traditional cement mortar is difficult to separate, resulting in high training costs and serious waste of resources in masonry projects, and it is difficult to achieve recycling.
A masonry adhesive was prepared by combining quicklime, gypsum powder, fly ash, carbonized garden waste, and propylene glycol block polyether. The masonry mortar was then treated with an aqueous acetic acid solution to facilitate its separation.
It achieves high strength and easy separation of masonry mortar, reduces resource waste, lowers costs, and enables the recycling of masonry materials.
Smart Images

Figure BDA0003984129850000061 
Figure BDA0003984129850000071 
Figure BDA0003984129850000072
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building materials, and in particular to a masonry adhesive and a preparation method and application thereof, a masonry mortar and a separation method thereof. Background Art
[0002] In recent years, in the construction of garden landscape, skilled technical personnel in masonry engineering are being vigorously cultivated. In the daily training of skilled technical personnel, masonry mortar is the main process material for masonry engineering, and the daily consumption is huge.
[0003] Traditional masonry mortar usually takes the form of cement mortar, which has many advantages such as good workability, high strength, and easy operation. However, due to the inherent hydraulic properties of cement mortar, the cement mortar will solidify into a whole after being used for masonry, and it is difficult to separate the cement mortar, which increases the training cost of masonry engineering. In addition, during the training process of masonry engineering, the difficult-to-separate cement mortar will cause a large amount of construction waste; and the masonry bricks are also contaminated and disabled by the cement mortar. The disabled masonry bricks will also generate a large amount of construction waste, which will lead to serious waste of resources and huge amount of waste.
[0004] At present, construction projects are basically using permanent bonding materials for masonry mortars, and there has been no improvement on this type of product from the perspective of recycling, which is also determined by the permanent characteristics of construction projects. However, in the actual application process, whether from the perspective of environmental protection or energy saving, as well as considering the overall cost control, making a masonry mortar that can be separated and then reused is of great significance and value for masonry training and temporary masonry projects. Summary of the invention
[0005] In order to reuse masonry mortar to meet the needs of masonry training and temporary masonry projects, the present application provides a masonry adhesive and a preparation method and application thereof, masonry mortar and a separation method thereof.
[0006] In a first aspect, the present application provides a masonry adhesive.
[0007] A masonry adhesive comprises the following components in parts by weight: 270-330 parts of quicklime; 180-220 parts of gypsum powder; 170-230 parts of fly ash; 50-80 parts of carbonized garden waste; and 5-9 parts of propylene glycol block polyether. The masonry adhesive does not contain cement.
[0008] The present application uses quicklime, gypsum powder, fly ash, carbonized products of garden waste and propylene glycol block polyether to make a masonry adhesive, and mixes the masonry adhesive with sand to obtain masonry mortar. The 28-day compressive strength of the masonry mortar obtained by the above method meets the strength requirements of masonry training and temporary masonry projects, and the masonry mortar can be easily separated after treatment for recycling and reuse.
[0009] The applicant has found through many tests that when cement is used, the masonry mortar obtained is difficult to separate. This is because the bonding effect of cement is very large. After use, the masonry mortar is not easy to break, and more fragments will remain. The diameter of the fragments is also large. Unless a more fine crushing process is performed, it is difficult to achieve reuse in conventional methods. Therefore, the masonry adhesive provided by this application does not contain cement.
[0010] Preferably, the method for preparing the carbonized product of garden waste is as follows: placing the garden waste at 400-600° C., carbonizing for 60-90 minutes, and crushing and sieving to obtain the carbonized product.
[0011] The present application utilizes garden waste such as tree branch clippings, lawn clippings, dead branches and leaves, weeds and dead flowers as resources. After carbonization, these garden wastes can be pyrolyzed and converted into a functional and environmentally friendly material with high organic carbon content, strong adsorption capacity and porosity. When used in masonry mortar, the compressive strength and separability of the masonry mortar can be improved.
[0012] Preferably, the average particle size of the carbonized product of garden waste is 15-20 um.
[0013] In a specific embodiment, the average particle size of the carbonized product of garden waste may be 15 um, 18 um, or 20 um.
[0014] In some specific embodiments, the average particle size of the carbonized product of garden waste may also be 15-18 um or 18-20 um.
[0015] Through experimental analysis, it is known that when the particle size of the carbonized product of garden waste is controlled within the range of 15-20um, the compressive strength of the masonry mortar can be further improved while ensuring that the masonry mortar is easy to separate. Therefore, the present application controls the particle size of the carbonized product of garden waste within the above range.
[0016] Preferably, the average molecular weight of the propylene glycol block polyether is 1600-2500.
[0017] In a specific embodiment, the average molecular weight of the propylene glycol block polyether can be 1600, 1630, 1900, or 2500.
[0018] In some specific embodiments, the average molecular weight of the propylene glycol block polyether may also be 1630-1900 or 1900-2500.
[0019] Furthermore, the viscosity of the propylene glycol block polyether at 25° C. is 250-440 cps.
[0020] In a specific embodiment, the viscosity of the propylene glycol block polyether at 25° C. may be 250 cps, 320 cps, 400 cps, or 440 cps.
[0021] In some specific embodiments, the viscosity of the propylene glycol block polyether at 25° C. may also be 250-320 cps or 320-400 cps.
[0022] The applicant has found that when propylene glycol block polyether is added to a masonry adhesive to prepare masonry mortar, not only can the compressive strength of the masonry mortar meet the requirements of masonry training, but the separability of the masonry mortar can also be greatly improved.
[0023] Through experimental analysis, it can be known that when the average molecular weight of the propylene glycol block polyether is within the above range and the viscosity at 25°C is within the above range, the compressive strength and separability of the masonry mortar can be further improved.
[0024] In a second aspect, the present application provides a method for preparing the above-mentioned masonry adhesive, which specifically comprises the following steps:
[0025] uniformly mixing the propylene glycol block polyether and water to obtain a propylene glycol block polyether aqueous solution;
[0026] The quicklime, the gypsum powder, the fly ash and the carbonized product of the garden waste are mixed and stirred to obtain a premix; the premix is added to the propylene glycol block polyether aqueous solution and mixed evenly to obtain the product.
[0027] The masonry adhesive obtained by the preparation method has good workability and is easy to construct during the process of preparing masonry mortar with sand.
[0028] In a third aspect, the present application provides a masonry mortar, comprising sand and the above-mentioned masonry adhesive.
[0029] Preferably, the weight ratio of the sand to the masonry adhesive is 3:(0.8-1.2).
[0030] In a fourth aspect, the present application provides a method for separating the above-mentioned masonry mortar, which specifically comprises the following steps:
[0031] Completely immersing the masonry mortar in an aqueous solution of acetic acid having a concentration of 3-5 wt %;
[0032] After 20-24 hours, the masonry mortar is taken out and placed at room temperature to dry;
[0033] Repeat the above steps until the masonry mortar reaches a state of automatic separation after vibration.
[0034] The present application found that the prepared masonry mortar was immersed in an acetic acid aqueous solution and then dried at room temperature; this was repeated several times and the mortar could be separated by vibration.
[0035] In a fifth aspect, the present application provides the use of the above-mentioned masonry adhesive or the above-mentioned masonry mortar in building materials.
[0036] The masonry adhesive and masonry mortar provided in this application can be reused to reduce costs and losses, reduce the amount of solid waste generated, truly kill two birds with one stone, and can effectively improve the problems currently faced by the construction industry in this field.
[0037] In summary, the technical solution of this application has the following effects:
[0038] The present application uses quicklime, gypsum powder, fly ash, carbonized products of garden waste and propylene glycol block polyether to make masonry mortar with sand. The 28-day compressive strength of the masonry mortar meets the strength requirements of masonry training and temporary masonry projects, and the masonry mortar can be easily separated after treatment for recycling and reuse.
[0039] The masonry mortar provided in the present application is soaked in an acetic acid aqueous solution and vibrated to be naturally separated.
[0040] The reusable masonry mortar provided in the present application can replace the traditional mortar, thereby achieving the multiple effects of recycling, environmental protection and energy saving. DETAILED DESCRIPTION
[0041] In a first aspect, the present application provides a masonry adhesive comprising the following components in parts by weight: 270-330 parts of quicklime; 180-220 parts of gypsum powder; 170-230 parts of fly ash; 50-80 parts of carbonized garden waste; 5-9 parts of propylene glycol block polyether; the masonry adhesive does not include cement.
[0042] The preparation method of the carbonized garden waste is as follows: placing the garden waste at 400-600°C, carbonizing for 60-90 minutes, crushing and sieving to obtain the carbonized garden waste; the average particle size of the carbonized garden waste is 15-20um.
[0043] Specifically, the average molecular weight of the propylene glycol block polyether is 1600-2500; and the viscosity at 25° C. is 250-440 cps.
[0044] In a second aspect, the present application provides a method for preparing the above-mentioned masonry adhesive, which specifically comprises the following steps:
[0045] Mixing the propylene glycol block polyether and water uniformly to obtain a propylene glycol block polyether aqueous solution;
[0046] The quicklime, gypsum powder, fly ash and carbonized product of garden waste are mixed and stirred to obtain a premix;
[0047] The premix is added into the propylene glycol block polyether aqueous solution and mixed evenly to obtain the product.
[0048] In a third aspect, the present application provides a masonry mortar, which includes sand and the above-mentioned masonry adhesive.
[0049] Among them, the weight ratio of sand to masonry adhesive is 3:(0.8-1.2).
[0050] In a fourth aspect, the present application provides a method for separating the above-mentioned masonry mortar, which specifically comprises the following steps:
[0051] The masonry mortar is completely immersed in an aqueous solution of acetic acid having a concentration of 3-5wt%;
[0052] After 20-24 hours, take out the masonry mortar and leave it to dry at room temperature;
[0053] Repeat the above steps until the masonry mortar reaches a state of automatic separation after vibration.
[0054] Propylene glycol block polyether was purchased from Hai'an Petrochemical Plant, Jiangsu Province. The remaining raw materials were commercially available.
[0055] The present application is further described in detail below in combination with preparation examples, embodiments, comparative examples and performance testing experiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0056] Preparation Example
[0057] Preparation Example 1
[0058] This preparation example provides a carbonized product of garden waste.
[0059] The preparation method of the carbonized product of garden waste in this preparation example is as follows:
[0060] The garden waste was placed in a high-temperature furnace, heated to 500°C at 5°C / min, carbonized for 75 minutes, then cooled to room temperature at 5°C / min, taken out, crushed and sieved to obtain the carbonized garden waste with an average particle size of 18um.
[0061] Preparation Example 2
[0062] This preparation example provides a carbonized product of garden waste.
[0063] The preparation method of the carbonized product of garden waste in this preparation example is as follows:
[0064] The garden waste was placed in a high-temperature furnace, heated to 500°C at 5°C / min, carbonized for 75 minutes, then cooled to room temperature at 5°C / min, taken out, crushed and sieved to obtain the carbonized garden waste with an average particle size of 10um.
[0065] Preparation Example 3
[0066] This preparation example provides a carbonized product of garden waste.
[0067] The preparation method of the carbonized product of garden waste in this preparation example is as follows:
[0068] The garden waste is placed in a high-temperature furnace, heated to 500°C at 5°C / min, carbonized for 75 minutes, then cooled to room temperature at 5°C / min, taken out, crushed and sieved to obtain the carbonized garden waste with an average particle size of 25um.
[0069] Preparation Example 4
[0070] This preparation example provides a masonry adhesive.
[0071] The carbonized product of garden waste in this preparation example comes from Preparation Example 1; the propylene glycol block polyether used is model L35, with an average molecular weight of 1900 and a viscosity of 320 cps at 25°C.
[0072] The preparation method of the masonry adhesive in this preparation example is:
[0073] Weigh 7 g of propylene glycol block polyether and mix evenly with 50 g of water to obtain a propylene glycol block polyether aqueous solution;
[0074] Weigh 300 g of quicklime, 200 g of gypsum powder, 210 g of fly ash, and 65 g of carbonized garden waste respectively, mix the four substances, and stir them evenly to obtain a premix;
[0075] The premix is added into the propylene glycol block polyether aqueous solution and stirred evenly to obtain a masonry adhesive.
[0076] Preparation Example 5
[0077] This preparation example provides a masonry adhesive.
[0078] The difference between this preparation example and preparation example 4 is that the carbonized product of garden waste comes from preparation example 2.
[0079] Preparation Example 6
[0080] This preparation example provides a masonry adhesive.
[0081] The difference between this preparation example and preparation example 4 is that the carbonized product of garden waste comes from preparation example 3.
[0082] Preparation Example 7
[0083] This preparation example provides a masonry adhesive.
[0084] The difference between this preparation example and preparation example 4 is that the added amount of propylene glycol block polyether is 5 g.
[0085] Preparation Example 8
[0086] This preparation example provides a masonry adhesive.
[0087] The difference between this preparation example and preparation example 4 is that the added amount of propylene glycol block polyether is 9 g.
[0088] Preparation Examples 9-12
[0089] Preparation Examples 9-12 each provide a masonry adhesive.
[0090] The difference between the above preparation example and preparation example 4 is that the type of propylene glycol block polyether is different, as shown in Table 1.
[0091] Table 1 Types of Preparation Examples 4, 9-12 Propylene glycol block polyethers
[0092]
[0093] Preparation Example 13
[0094] This preparation example provides a masonry adhesive.
[0095] The difference between this preparation example and preparation example 4 is that the masonry adhesive does not contain carbonized products of garden waste.
[0096] The preparation method of the masonry adhesive in this preparation example is:
[0097] Weigh 7 g of propylene glycol block polyether and mix evenly with 50 g of water to obtain a propylene glycol block polyether aqueous solution;
[0098] Weigh 300 g of quicklime, 200 g of gypsum powder, and 210 g of fly ash respectively, mix the three substances, and stir them evenly to obtain a premix;
[0099] The premix is added into the propylene glycol block polyether aqueous solution and stirred evenly to obtain a masonry adhesive.
[0100] Preparation Example 14
[0101] This preparation example provides a masonry adhesive.
[0102] This Preparation Example is different from Preparation Example 4 in that the masonry adhesive does not contain propylene glycol block polyether.
[0103] The preparation method of the masonry adhesive in this preparation example is:
[0104] Weigh 300 g of quicklime, 200 g of gypsum powder, 210 g of fly ash, and 65 g of carbonized garden waste respectively, mix the four substances, and stir them evenly to obtain a premix;
[0105] The premix was added into 57 g of water and stirred evenly to obtain a masonry adhesive.
[0106] Preparation Example 15
[0107] This preparation example provides a masonry adhesive.
[0108] This Preparation Example is different from Preparation Example 4 in that the masonry adhesive further contains 100 parts of cement.
[0109] Weigh 7 g of propylene glycol block polyether and mix evenly with 50 g of water to obtain a propylene glycol block polyether aqueous solution;
[0110] Weigh 300 g of quicklime, 200 g of gypsum powder, 210 g of fly ash, 100 g of cement, and 65 g of carbonized garden waste respectively, mix the four substances, and stir them evenly to obtain a premix;
[0111] The premix is added into the propylene glycol block polyether aqueous solution and stirred evenly to obtain a masonry adhesive.
[0112] Preparation Example 16
[0113] This preparation example provides a masonry adhesive.
[0114] The difference between this preparation example and preparation example 4 is that the added amount of propylene glycol block polyether is 3 g.
[0115] Preparation Example 17
[0116] This preparation example provides a masonry adhesive.
[0117] The difference between this preparation example and preparation example 4 is that the added amount of propylene glycol block polyether is 10 g.
[0118] Example
[0119] Examples 1-9
[0120] Examples 1-9 each provide a masonry mortar.
[0121] The difference between the above embodiments is that the types of masonry adhesives are specifically shown in Table 2.
[0122] The preparation method of the separable masonry mortar in the above embodiment is:
[0123] Mix sand and masonry adhesive in a weight ratio of 3:1 to obtain;
[0124] Among them, the average particle size of sand is 0.25mm-0.5mm; the mud content is ≤2.5% and the water content is ≤2%.
[0125] Table 2 Types of masonry adhesives in Examples 1-9
[0126]
[0127] Comparative Example
[0128] Comparative Examples 1-5
[0129] The above comparative example provides a masonry mortar.
[0130] The difference between the above comparative examples is: the type of masonry adhesive, as shown in Table 3.
[0131] Table 3 Types of masonry adhesives in Comparative Examples 1-5
[0132]
[0133] Performance testing
[0134] Test Example 1
[0135] This test example examined the compressive strength of masonry mortar.
[0136] According to the method of JGJ / T70-2009 "Standard for Test Methods for Basic Properties of Building Mortar", the masonry mortars prepared in Examples 1-9 and Comparative Examples 1-5 were cast into masonry mortar specimens and allowed to stand at 20°C for 24 hours. After the test pieces were demoulded, they were allowed to stand at 20°C for standard curing for 28 days.
[0137] The compressive strength of the above masonry mortar was tested.
[0138] Test results: as shown in Table 4.
[0139] Test Example 2
[0140] This test example examined the separability of masonry mortar.
[0141] The masonry mortar specimens in Test Example 1 were completely immersed in an acetic acid aqueous solution having a concentration of 4 wt %;
[0142] After 24 h, the masonry mortar specimens were taken out and dried at room temperature for 4 h;
[0143] Repeat the above steps until the masonry mortar specimen reaches a state of automatic separation after vibration.
[0144] Test results: as shown in Table 4.
[0145] Table 4 Performance test results of masonry mortar in Examples 1-9 and Comparative Examples 1-5
[0146]
[0147] Combined with Table 4, by comparing the test results of Examples 1-9 with Comparative Examples 1-5, it can be seen that the present application uses quicklime, gypsum powder, fly ash, carbonized products of garden waste and propylene glycol block polyether to make a masonry adhesive, and mixes the masonry adhesive with sand to obtain a masonry mortar. The 28-day compressive strength of the masonry mortar obtained by the above method meets the strength requirements of masonry training, and the masonry mortar is treated with an acetic acid aqueous solution and can be easily separated and recycled.
[0148] By comparing the test results of Example 1 with Comparative Example 1, when the carbonized product of garden waste is not used, the compressive strength of the masonry mortar is low and cannot meet the requirements of masonry training; and the masonry mortar is difficult to separate. Further, by comparing the test results of Examples 1-3, when the particle size of the carbonized product of garden waste is controlled within the range of 15-20um, the compressive strength of the masonry mortar can be further improved. Therefore, the present application selects to use the carbonized product of garden waste for preparing masonry mortar, and controls the particle size of the carbonized product of garden waste within the above range.
[0149] By comparing the test results of Example 1 with those of Comparative Example 3, when the masonry adhesive also contains 100 parts of cement, the masonry mortar cannot be separated. Therefore, cement is not used to prepare masonry mortar in this application.
[0150] By comparing the test results of Example 1 with Comparative Example 2, when propylene glycol block polyether is not used, the masonry mortar cannot be separated. Further, by comparing the test results of Example 1, Examples 4-5 and Comparative Examples 4-5, when the amount of propylene glycol block polyether added is less than 5 parts, the masonry mortar separation cycle is too long, increasing the test cost; and when the amount of propylene glycol block polyether added is more than 9 parts, the compressive strength of the masonry mortar is low and cannot meet the requirements of masonry training.
[0151] By comparing the test results of Example 1 with those of Examples 6-9, when the average molecular weight of the propylene glycol block polyether is 1600-2500 and the viscosity at 25° C. is 250-440 cps, the compressive strength and separability of the masonry mortar can be further improved.
[0152] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A masonry adhesive, It is characterized in that The invention is composed of the following components in parts by weight: 270-330 parts of quicklime; 180-220 parts of gypsum powder; 170-230 parts of fly ash; 50-80 parts of carbonized garden waste; 5-9 parts of propylene glycol block polyether; the masonry adhesive does not include cement; The average molecular weight of the propylene glycol block polyether is 1900-2500, and the viscosity at 25° C. is 320-440 cps.
2. The masonry adhesive according to claim 1, It is characterized in that The preparation method of the carbonized product of garden waste is as follows: placing the garden waste under the condition of 400-600° C., carbonizing for 60-90 minutes, and crushing and sieving to obtain the carbonized product.
3. The masonry adhesive according to claim 1, It is characterized in that The average particle size of the carbonized product of garden waste is 15-20 microns.
4. A method for preparing a masonry adhesive according to any one of claims 1 to 3, It is characterized in that The specific steps include: uniformly mixing the propylene glycol block polyether and water to obtain a propylene glycol block polyether aqueous solution; The quicklime, the gypsum powder, the fly ash and the carbonized product of the garden waste are mixed and stirred to obtain a premix; The premix is added into the propylene glycol block polyether aqueous solution and mixed evenly to obtain the product.
5. A masonry mortar, It is characterized in that The invention comprises sand and the masonry adhesive according to any one of claims 1 to 3.
6. The masonry mortar according to claim 5, It is characterized in that The weight ratio of the sand to the masonry adhesive is 3:(0.8-1.2).
7. A method for separating masonry mortar according to any one of claims 5 to 6, It is characterized in that The specific steps include: The masonry mortar is completely immersed in an acetic acid aqueous solution having a concentration of 3-5wt%; After 20-24 hours, the masonry mortar is taken out and placed at room temperature to dry; Repeat the above steps until the masonry mortar reaches a state of automatic separation after vibration.