Small-grain SAPO-34 molecular sieve, preparation method and application thereof, and method for preparing olefins from methanol
By pretreating the aluminum source and high-silica SAPO-34 molecular sieve in the presence of template agent and water, and adding the silicon source and phosphorus source under hydrothermal conditions, a small-grained SAPO-34 molecular sieve was prepared, solving the problems in the existing technology. Efficient catalytic performance and industrial applications were achieved using expensive additives and large grain sizes.
Patent Information
- Application Number
- CN202111453652.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-12-01
AI Technical Summary
The preparation process of small and medium-sized SAPO-34 molecular sieves in the prior art requires the use of expensive template agents or other additives, which results in high production costs, complex synthesis processes and difficult to control product composition. In addition, the molecular sieves have large crystal size, which affects the catalytic performance. .
The initial gel is formed by mixing aluminum source, high-silica SAPO-34 molecular sieve, template agent and water, and pre-treated in the presence of template agent and water, and then added silicon source and phosphorus source for hydrothermal crystallization and roasting. The small-grained SAPO-34 molecular sieve is obtained, avoiding the use of expensive template agents, achieving uniform particle size distribution and high synthesis yield.
The uniform particle size (0.5-1.5 μm) and high synthesis yield (greater than 80%) of the small-grained SAPO-34 molecular sieve are achieved, which extends the life of the catalyst and improves the selectivity of low-carbon olefins, making it suitable for industrial applications.
Smart Images

Figure CN116199237B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of molecular sieves, and in particular to a small-grain SAPO-34 molecular sieve and a preparation method and application thereof. Background Art
[0002] In 1984, the United Carbide Corporation (UCC) of the United States developed the silicoaluminophosphate series molecular sieve (SAPO). This molecular sieve is a type of crystalline silicoaluminophosphate, and its three-dimensional framework structure is composed of PO 2+ 、AlO 2- and SiO2 tetrahedron. Among them, the framework structure of SAPO-34 is CHA structure, and the main pore is an octahedral ring structure. Due to its suitable acidity and pore structure, it exhibits excellent catalytic performance in the methanol to olefins (MTO) reaction and is currently the most widely used MTO catalyst.
[0003] However, due to its small pores and large cage structure, SAPO-34 molecular sieve is prone to rapid carbon deposition and deactivation in the MTO reaction. At the same time, it also has the problem of limited diffusion during the reaction, which leads to a decrease in catalytic performance.
[0004] The reduction of molecular sieve particle size can not only increase the external specific surface area and the number of pores on the surface, thereby improving the specific activity of the molecular sieve, but also shorten the diffusion path of reactants and products, weaken the diffusion restriction, and thus improve the catalyst's ability to resist carbon deposition and extend the catalyst life. At present, the average particle size of SAPO-34 molecular sieve synthesized by conventional methods is generally 5-20μm. How to effectively reduce the particle size of SAPO-34 molecular sieve is a hot topic of current research.
[0005] CN104340986A discloses a method for preparing small-grain SAPO-34 molecular sieve, which comprises pre-treating the SAPO-34 molecular sieve into particles with a particle size of 10-800 nm as a crystallization precursor; mixing an organic amine template and water as well as an optional silicon source, aluminum source and phosphorus source to prepare a crystallization liquid, subjecting the crystallization precursor and the crystallization liquid to hydrothermal crystallization, and finally separating to obtain small-grain SAPO-34 molecular sieve.
[0006] CN104445266A discloses a method for preparing a small-grain SAPO-34 molecular sieve, which mainly solves the problem of large grain size of SAPO-34 molecular sieve obtained by traditional synthesis method, and is characterized by promoting the synthesis of small-grain molecular sieve by adding crystal seeds with defective structure. The technical scheme mainly comprises: 1. hydrothermally crystallizing the initial crystallization liquid of SAPO-34 molecular sieve at 200-250°C for 1-10h, and obtaining SAPO-34 crystal seeds with more lattice defects after solid-liquid separation; 2. adding this crystal seed to the initial crystallization liquid of SAPO-34, and after hydrothermal treatment at 140-170°C for 0.1-4h, it can be dissolved into fine fragments that ultimately play a structural guiding and nucleation role, and then heating to 180-250°C to continue hydrothermal crystallization to obtain a small-grain SAPO-34 molecular sieve product.
[0007] CN105585022A discloses a method for preparing sheet-like nano SAPO-34 molecular sieves, which comprises adding specific organic additives to a gel mixed with an aluminum source, a phosphorus source, a silicon source, a template and water, stirring evenly, adding the nano SAPO-34 molecular sieve as a seed, and preparing the sheet-like nano SAPO-34 molecular sieve by variable temperature crystallization.
[0008] The defects in the preparation of small-grain SAPO-34 molecular sieves in the prior art, especially in the process of industrial application, mainly include: (1) the use of tetraethylammonium hydroxide (TEAOH) as a template or the addition of specific organic additives, which greatly increases the production cost; (2) the synthesis process is complicated, the composition of the final product is difficult to control, and the molecular sieve synthesis yield is low. Summary of the invention
[0009] The purpose of the present invention is to overcome the problem that a specific template or other auxiliary agent is required in the process of preparing a small-grain SAPO-34 molecular sieve in the prior art, and the grain size of the obtained SAPO-34 molecular sieve is large, and to provide a small-grain SAPO-34 molecular sieve and a preparation method and application thereof, wherein the preparation method does not require the addition of expensive templates or other organic additives, the process is easy to operate, and it is easy to realize industrial application. The preparation method can obtain a small-grain molecular sieve with uniform particle size distribution while greatly improving the synthesis yield of the molecular sieve.
[0010] In order to achieve the above object, the first aspect of the present invention provides a method for preparing small-grain SAPO-34 molecular sieve, characterized in that the method comprises the following steps:
[0011] (1) mixing an aluminum source, a high-silicon SAPO-34 molecular sieve, a template agent and water and performing pretreatment to obtain an initial gel;
[0012] (2) The initial gel is mixed with a silicon source and a phosphorus source to obtain a mixed solution, and the mixed solution is aged, hydrothermally crystallized, and calcined to obtain the small-grain SAPO-34 molecular sieve.
[0013] The second aspect of the present invention provides a small-grain SAPO-34 molecular sieve prepared by the above preparation method.
[0014] A third aspect of the present invention provides an application of the small-grain SAPO-34 molecular sieve in methanol to olefins.
[0015] A fourth aspect of the present invention provides a method for preparing olefins from methanol, characterized in that the method comprises: in the presence of a protective gas, methanol and a molecular sieve are contacted and reacted;
[0016] The molecular sieve is the above-mentioned small-grain SAPO-34 molecular sieve.
[0017] Through the above technical scheme, the small-grain SAPO-34 molecular sieve and its preparation method and application, and the method for preparing methanol to olefins provided by the present invention achieve the following beneficial effects:
[0018] In the present invention, an aluminum source and a high-silicon SAPO-34 molecular sieve are pretreated in the presence of a template and water, and the ratio of the template and water is controlled to form a primary structure for constructing a molecular sieve framework and an initial gel of active elements. On this basis, a silicon source and a phosphorus source are further added for crystallization to obtain a small-grain SAPO-34 molecular sieve.
[0019] Furthermore, the small-grain SAPO-34 molecular sieve provided by the present invention has an average particle size of 0.5-1.5 μm, and the molecular sieve crystal size is uniform, and has a high molecular sieve synthesis yield, the molecular sieve synthesis yield is greater than 80%, and it is easy to achieve industrial application. When it is used in the methanol to olefin reaction, it can show a long catalytic life and a high selectivity for light olefins. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 X-ray diffraction (XRD) patterns of the molecular sieves prepared in Examples 1-3 and Comparative Examples 1-3;
[0021] Figure 2 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Example 1;
[0022] Figure 3 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Example 2;
[0023] Figure 4 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Example 3;
[0024] Figure 5 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Example 8;
[0025] Figure 6 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Comparative Example 1;
[0026] Figure 7 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Comparative Example 2;
[0027] Figure 8 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Comparative Example 3;
[0028] Fig. 9 This is a scanning electron microscope photo (SEM) of the molecular sieve prepared in Comparative Example 4;
[0029] Fig.10 This is a scanning electron microscope photograph (SEM) of the molecular sieve prepared in Comparative Example 5. DETAILED DESCRIPTION
[0030] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0031] The first aspect of the present invention provides a method for preparing a small-grain SAPO-34 molecular sieve, characterized in that the method comprises the following steps:
[0032] (1) mixing an aluminum source, a high-silicon SAPO-34 molecular sieve, a template agent and water and performing pretreatment to obtain an initial gel;
[0033] (2) The initial gel is mixed with a silicon source and a phosphorus source to obtain a mixed solution, and the mixed solution is aged, hydrothermally crystallized, and calcined to obtain the small-grain SAPO-34 molecular sieve.
[0034] In the present invention, an aluminum source and a high-silicon SAPO-34 molecular sieve are pretreated in the presence of a template and water, and the ratio of the template and water is controlled to form a primary structure for constructing a molecular sieve framework and an initial gel of active elements, and on this basis, a silicon source and a phosphorus source are further added for crystallization, so that a small-grain SAPO-34 molecular sieve can be prepared, and the molecular sieve has a high synthesis yield.
[0035] According to the present invention, the Si / Al ratio of the high-silicon SAPO-34 molecular sieve is 0.4-0.6.
[0036] In the present invention, the SAPO-34 molecular sieve having the above Si / Al is used, which can form an effective active unit or primary structure under alkaline conditions in the presence of a template and water, and can play a seed-guiding role while providing a portion of the Si source, thereby inducing the synthesis of small-grain SAPO-34 molecular sieves.
[0037] According to the present invention, the amount of the aluminum source, the high silicon SAPO-34 molecular sieve, the template, the water, the silicon source and the phosphorus source is such that the molar ratio of the components in the mixed solution is: aR:bSiO2:Al2O3:cP2O5:dH2O, wherein R is the template, 0.5≤a≤8; 0.1≤b≤1; 0.1≤c≤2.5; 5≤d≤20; 0.3
[0038] Furthermore, the amounts of the aluminum source, the high silicon SAPO-34 molecular sieve, the template, the water, the silicon source and the phosphorus source are such that the molar ratio of the components in the mixed solution is: aR:bSiO2:Al2O3:cP2O5:dH2O, wherein R is the template, 2≤a≤6; 0.2≤b≤0.5; 0.8≤c≤1.5; 10≤d≤15; 0.4
[0039] According to the present invention, the pretreatment temperature is 30-80°C, and the pretreatment time is 2-48h.
[0040] In the present invention, under the above conditions, a mixture containing an aluminum source, a high-silicon SAPO-34 molecular sieve, a template and water is pretreated to activate the reaction precursors to form silicon and aluminum primary units with higher reaction activity, thereby obtaining a SAPO-34 molecular sieve with small crystals and high yield.
[0041] Furthermore, the pretreatment temperature is 40-70° C., and the pretreatment time is 12-36 hours.
[0042] According to the present invention, the aging conditions include: aging time of 2-48h, aging temperature of 30-80°C.
[0043] Furthermore, the aging conditions include: aging time of 6-24h, aging temperature of 40-60°C.
[0044] According to the present invention, the hydrothermal crystallization conditions include: a hydrothermal crystallization temperature of 170-210° C., and a hydrothermal crystallization time of 6-40 h.
[0045] Furthermore, the conditions for the hydrothermal crystallization include: a hydrothermal crystallization temperature of 180-200° C., and a hydrothermal crystallization time of 6-40 h.
[0046] According to the present invention, the calcination conditions include: a calcination temperature of 500-700° C. and a calcination time of 2-12 hours.
[0047] Furthermore, the calcination conditions include: a calcination temperature of 550-650° C. and a calcination time of 6-8 hours.
[0048] According to the present invention, the phosphorus source is selected from at least one of phosphoric acid, phosphorous acid and phosphorus pentoxide.
[0049] According to the present invention, the aluminum source is selected from at least one of pseudo-boehmite, aluminum sol and aluminum isopropoxide.
[0050] In the present invention, the content of aluminum oxide in the aluminum sol is 10-30wt%.
[0051] According to the present invention, the silicon source is selected from at least one of silica sol, tetraethyl orthosilicate and active silicon dioxide.
[0052] In the present invention, the content of silicon dioxide in the silica sol is 10-40wt%.
[0053] According to the present invention, the template agent is at least one selected from triethylamine, diisopropylamine, diethylamine, morpholine, N,N-diisopropylethylamine, cyclohexylamine and n-butylamine.
[0054] In the present invention, the method further comprises: washing, filtering and drying the product after hydrothermal crystallization with deionized water. The specific operation steps and conditions of washing, filtering and drying can be carried out according to conventional steps in the art.
[0055] In one specific embodiment of the present invention, the small-grain SAPO-34 molecular sieve is prepared according to the following steps:
[0056] (1) After the aluminum source, high-silicon SAPO-34 molecular sieve and water are uniformly mixed, a template is added, and after stirring at 20-60° C. for 0.5-36 hours, the mixture is transferred into a reaction kettle with a polytetrafluoroethylene lining for pretreatment to obtain an initial gel;
[0057] (2) After the initial gel is cooled to room temperature, a silicon source is added under stirring, and the stirring is continued for 0.5-24 hours. Then, a phosphorus source is added, and the stirring is continued for 0.5-24 hours to obtain a mixed solution, and the mixed solution is aged and hydrothermally crystallized. The product after hydrothermal crystallization is washed with deionized water, filtered, and dried, and then calcined in an air atmosphere to obtain the small-grain SAPO-34 molecular sieve.
[0058] The second aspect of the present invention provides a small-grain SAPO-34 molecular sieve prepared by the above preparation method.
[0059] According to the present invention, the average particle size of the small-grain SAPO-34 molecular sieve is 0.5-1.5 μm.
[0060] In the present invention, the average particle size of the small-grain SAPO-34 molecular sieve is 0.5-1.5 μm, and the molecular sieve crystal size is uniform, which is easy to realize industrial application. When it is used in the methanol to olefin reaction, it can show a longer catalytic life and higher selectivity for light olefins.
[0061] Furthermore, the average particle size of the small-grain SAPO-34 molecular sieve is 0.5-1 μm.
[0062] A third aspect of the present invention provides an application of the small-grain SAPO-34 molecular sieve in methanol to olefins.
[0063] When the small-grain SAPO-34 molecular sieve of the present invention is used in a methanol to olefin reaction, it can exhibit a longer catalytic life and higher selectivity for light olefins.
[0064] A fourth aspect of the present invention provides a method for preparing olefins from methanol, characterized in that the method comprises: in the presence of a protective gas, methanol and a molecular sieve are contacted and reacted;
[0065] The molecular sieve is the above-mentioned small-grain SAPO-34 molecular sieve.
[0066] In the present invention, the contact reaction conditions include: reaction temperature of 400-500°C, reaction pressure of 0-0.2MPa, methanol space velocity of 1-10h -1 .
[0067] In the present invention, the protective gas may be a conventional protective gas in the art, such as nitrogen.
[0068] The present invention will be described in detail below by way of examples. In the following examples,
[0069] The average particle size of small-grain SAPO-34 molecular sieve was measured by laser particle size method, and the testing instrument was Malvern Mastersizer 3000 laser diffraction particle size analyzer;
[0070] The morphology of small-grain SAPO-34 molecular sieve was characterized by scanning electron microscopy (SEM);
[0071] The crystal form of small-grain SAPO-34 molecular sieve was measured by X-ray diffraction (XRD);
[0072] The synthesis yield of small-grain SAPO-34 molecular sieve is calculated according to the following method:
[0073] Molecular sieve synthesis yield = product dry weight / raw material oxide dry weight × 100%;
[0074] The raw materials used in the examples and comparative examples are all commercially available.
[0075] Example 1
[0076] (1) 10 g of pseudo-boehmite and 0.5 g of high-silicon SAPO-34 (Si / Al=0.5) molecular sieve were mixed evenly with 8 g of deionized water, 40.48 g of triethylamine was added, and after stirring at room temperature for 2 h, the mixture was transferred into a reaction kettle with a polytetrafluoroethylene liner and treated at 60° C. for 24 h.
[0077] (2) After the pretreated mixed gel is cooled to room temperature, 3.41 g of silica sol (30 wt%) is added under stirring. After stirring for 1 hour, 14.83 g of phosphoric acid (85 wt%) is added dropwise. After stirring for 1 hour, a mixed solution is obtained. The mixed solution is aged at room temperature for 2 hours and crystallized at 200°C for 24 hours. The obtained product is washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650°C in an air atmosphere for 5 hours to obtain small-grain SAPO-34 molecular sieve A1. The synthetic yield of the molecular sieve is 87%. The molar ratio of the components in the mixed solution is: 6R: 0.26SiO2: Al2O3: 0.96P2O5: 13H2O, where a / d is 0.46.
[0078] The XRD spectrum of small-grain SAPO-34 molecular sieve A1 is shown in Figure 1 As shown, the microscopic morphology is Figure 2 As shown in the SEM photograph, the SAPO-34 molecular sieve has a cubic morphology and a uniform particle size with an average particle size of 0.5 μm.
[0079] from Figure 1 It can be seen that the sample prepared in Example 1 exhibits characteristic diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, and 25.1±0.1°, indicating that the prepared sample is a SAPO-34 molecular sieve with a CHA topological structure.
[0080] Example 2
[0081] (1) 10 g of pseudo-boehmite and 0.86 g of high-silicon SAPO-34 (Si / Al=0.6) molecular sieve were mixed evenly with 8 g of deionized water, 36.55 g of diisopropylamine was added, and after stirring at room temperature for 2 h, the mixture was transferred into a reaction kettle with a polytetrafluoroethylene liner and treated at 70° C. for 16 h.
[0082] (2) After the pretreated mixed gel is cooled to room temperature, 3.41 g of silica sol (30 wt%) is added under stirring. After stirring for 1 hour, 14.08 g of phosphoric acid (85 wt%) is added dropwise. After stirring for 1 hour, a mixed solution is obtained. The mixed solution is aged at room temperature for 2 hours and crystallized at 200°C for 30 hours. The obtained product is washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650°C in an air atmosphere for 5 hours to obtain small-grain SAPO-34 molecular sieve A2. The synthetic yield of the molecular sieve is 83%. The molar ratio of the components in the mixed solution is: 5.4R: 0.26SiO2: Al2O3: 0.96P2O5: 13H2O, where a / d is 0.42.
[0083] The XRD spectrum of small-grain SAPO-34 molecular sieve A2 is shown in Figure 1 As shown, the microscopic morphology is Figure 3 As shown in the SEM photograph, the SAPO-34 molecular sieve has a cubic morphology and a uniform particle size with an average particle size of 0.65 μm.
[0084] from Figure 1 It can be seen that the sample prepared in Example 2 shows characteristic diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, and 25.1±0.1°, indicating that the prepared sample is a SAPO-34 molecular sieve with a CHA topological structure.
[0085] Example 3
[0086] (1) 27.24 g of aluminum isopropoxide and 0.45 g of high-silicon SAPO-34 (Si / Al=0.5) molecular sieve were mixed evenly with 8 g of deionized water, 40.48 g of triethylamine was added, and after stirring at room temperature for 2 h, the mixture was transferred into a reaction kettle with a polytetrafluoroethylene liner and treated at 70° C. for 12 h.
[0087] (2) After the pretreated mixed gel is cooled to room temperature, 3.41 g of silica sol (30%) is added under stirring. After stirring for 1 hour, 14.83 g of phosphoric acid (85%) is added dropwise. Stirring is continued for 1 hour to obtain a mixed solution. The mixed solution is aged at room temperature for 2 hours and crystallized at 200°C for 24 hours. The obtained product is washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650°C in an air atmosphere for 5 hours to obtain small-grain SAPO-34 molecular sieve A3. The synthetic yield of the molecular sieve is 84%. The molar ratio of the components in the mixed solution is: 6R: 0.26SiO2: Al2O3: 0.96P2O5: 13H2O, where a / d is 0.46.
[0088] The XRD spectrum of small-grain SAPO-34 molecular sieve A3 is shown in Figure 1 As shown, the microscopic morphology is Figure 4As shown in the SEM photograph, the SAPO-34 molecular sieve has a cubic morphology and a uniform particle size with an average particle size of 0.55 μm.
[0089] from Figure 1 It can be seen that the sample prepared in Example 3 shows characteristic diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, and 25.1±0.1°, indicating that the prepared sample is a SAPO-34 molecular sieve with a CHA topological structure.
[0090] Example 4
[0091] (1) 10 g of pseudo-boehmite and 0.90 g of high-silicon SAPO-34 molecular sieve (Si / Al=0.6) were mixed evenly with 8 g of deionized water, and 35.21 g of triethylamine (R1) and 3.90 g of diethylamine (R2) were added. After stirring at room temperature for 2 h, the mixture was transferred into a reaction kettle with a polytetrafluoroethylene liner and treated at 60° C. for 24 h.
[0092] (2) After the pretreated mixed gel is cooled to room temperature, 6.05 g of silica sol (30 wt%) is added under stirring. After stirring for 1 hour, 15.26 g of phosphoric acid (85%) is added dropwise. After stirring for 1 hour, a mixture is obtained. The mixed solution is aged at room temperature for 2 hours and crystallized at 200°C for 16 hours. The obtained product is washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650°C in an air atmosphere for 5 hours to obtain small-grain SAPO-34 molecular sieve A4. The synthetic yield of the molecular sieve is 85%. The molar ratio of each component material in the mixed solution is: 5.2R1: 0.8R2: 0.30SiO2: Al2O3: 0.85P2O5: 13.3H2O, wherein a / d = 0.45 ((0.52 + 0.8) / 13.3 = 0.45).
[0093] Small-grain SAPO-34 molecular sieve A5 has a cubic structure with an average particle size of about 1 μm.
[0094] Example 5
[0095] (1) 10 g of pseudo-boehmite and 1 g of high-silicon SAPO-34 molecular sieve (Si / Al=0.6) were mixed evenly with 8.50 g of deionized water, 32.21 g of triethylamine was added, and after stirring at room temperature for 2 h, the mixture was transferred into a reaction kettle with a polytetrafluoroethylene liner and treated at 60° C. for 24 h.
[0096] (2) After the pretreated mixed gel is cooled to room temperature, 3.50 g of tetraethyl orthosilicate is added under stirring. After stirring for 1 hour, 16.26 g of phosphoric acid (85 wt%) is added dropwise. After stirring for 1 hour, a mixed solution is obtained. The mixed solution is aged at room temperature for 2 hours and crystallized at 200°C for 36 hours. The obtained product is washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650°C in an air atmosphere for 5 hours to obtain small-grain SAPO-34 molecular sieve A5. The synthetic yield of the molecular sieve is 82%. The molar ratio of the components in the mixed solution is: 4.8R: 0.25SiO2: Al2O3: 1.05P2O5: 11.8H2O, where a / d = 0.41.
[0097] The small-grain SAPO-34 molecular sieve A5 has a cubic structure with an average particle size of 0.8 μm.
[0098] Example 6
[0099] The same method as in Example 1 was used to prepare the SAPO-34 molecular sieve, except that the Si / Al ratio of the high-silicon SAPO-34 molecular sieve was changed to 0.3, and the other conditions remained unchanged to obtain molecular sieve A6, with a synthetic yield of 82%. Molecular sieve A6 was a cubic structure with an average particle size of 1.2 μm.
[0100] Example 7
[0101] The same method as in Example 1 was used to prepare the SAPO-34 molecular sieve, except that the Si / Al ratio of the high-silicon SAPO-34 molecular sieve was changed to 0.7, and the other conditions remained unchanged to obtain molecular sieve A7, with a synthetic yield of 83%. Molecular sieve A7 was a cubic structure with an average particle size of 1.3 μm.
[0102] Example 8
[0103] The same method as in Example 1 was used to prepare SAPO-34 molecular sieve, except that the pretreatment conditions were changed to: treatment at 100°C for 60 hours, and the other conditions remained unchanged to obtain molecular sieve A8, with a synthetic yield of 83%. The microscopic morphology of SAPO-34 molecular sieve A8 is shown in Figure 5 As shown in the SEM photograph, the average particle size of the SAPO-34 molecular sieve is 1.5 μm and has a cubic morphology. When the particle size of the molecular sieve A9 is tested using a laser diffraction particle size analyzer, the particle size shows a bimodal distribution, indicating that the particle size distribution is uneven.
[0104] Example 9
[0105] The same method as in Example 1 was used to prepare the SAPO-34 molecular sieve, except that the addition amount of the high silicon SAPO-34 molecular sieve was changed to 1.5 g, and the molar ratio of the components in the mixed solution was: 6R: 0.20SiO2: Al2O3: 0.95P2O5: 13H2O, wherein a / d was 0.46, and the conditions were unchanged to obtain the molecular sieve A9, and the synthesis yield of the molecular sieve was 80%. The molecular sieve A9 had a cubic structure with an average particle size of 1.5 μm. When the particle size of the molecular sieve A9 was tested by a laser diffraction particle size analyzer, the particle size showed a bimodal distribution, indicating that the particle size distribution was uneven.
[0106] Comparative Example 1
[0107] Preparation of SAPO-34 molecular sieve by traditional hydrothermal synthesis
[0108] 10g of pseudo-boehmite, 14.88g of phosphoric acid (concentration of 85wt%) and 47.23g of deionized water were mixed and stirred. After stirring for 1 hour, 7.71g of silica sol (SiO2 content of 30wt%) was added dropwise. After stirring evenly, 19.65g of template triethylamine was added, and stirring was continued for 1h. The mixture was aged at room temperature for 2h. The molar ratio of each component in the obtained mixture was: 3R: 0.6SiO2: 1Al2O3: 1P2O5: 50H2O, wherein a / d was 0.06. The above gel was placed in a reactor with a polytetrafluoroethylene lining, and hydrothermally crystallized at 200℃ for 48 hours. The obtained product was centrifugally washed with deionized water, filtered, and dried, and then calcined at 650℃ in an air atmosphere for 5 hours to obtain SAPO-34 molecular sieve D1. The synthetic yield of the molecular sieve was 48%.
[0109] The XRD spectrum of SAPO-34 molecular sieve D1 is as follows Figure 1 As shown, the microscopic morphology is Figure 6 As shown in the SEM photograph, the SAPO-34 molecular sieve has a cubic morphology and an average particle size of 7 μm.
[0110] from Figure 1 It can be seen that the sample prepared in Comparative Example 1 shows characteristic diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, and 25.1±0.1°, indicating that the prepared sample is a SAPO-34 molecular sieve with a CHA topological structure.
[0111] Comparative Example 2
[0112] The batching process and proportions were the same as those in Example 1, but high-silicon SAPO-34 molecular sieve was not added.
[0113] (1) 10 g of pseudo-boehmite was mixed with 8 g of deionized water, 40.48 g of triethylamine was added, and the mixture was stirred at room temperature for 2 h. The mixture was then transferred into a polytetrafluoroethylene-lined reactor and treated at 60° C. for 24 h.
[0114] (2) After the pretreated mixed gel is cooled to room temperature, 3.41 g of silica sol (30 wt%) is added under stirring. After stirring for 1 hour, 14.83 g of phosphoric acid (85 wt%) is added dropwise. After stirring for 1 hour, a mixed solution is obtained. The mixed solution is aged at room temperature for 2 hours and crystallized at 200°C for 24 hours. The obtained product is washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650°C in an air atmosphere for 5 hours to obtain SAPO-34 molecular sieve D2. The synthetic yield of the molecular sieve is 51%. The molar ratio of the components in the mixed solution is: 6R: 0.26SiO2: Al2O3: 0.96P2O5: 13H2O, wherein a / d is 0.46.
[0115] The XRD spectrum of SAPO-34 molecular sieve D2 is as follows Figure 1 As shown, the microscopic morphology is Figure 7 As shown in the SEM photograph, the SAPO-34 molecular sieve has a cubic morphology, uneven particle size, and an average particle size of 4.5 μm.
[0116] from Figure 1 It can be seen that the sample prepared in Comparative Example 2 shows characteristic diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, and 25.1±0.1°, indicating that the prepared sample is a SAPO-34 molecular sieve with a CHA topological structure.
[0117] Comparative Example 3
[0118] The proportion of ingredients is the same as that in Example 1, but no pretreatment is performed.
[0119] 10g pseudo-boehmite and 0.5g high silicon SAPO-34 (Si / Al=0.5) molecular sieve were mixed evenly with 8g deionized water, 40.48g triethylamine was added, and after stirring at room temperature for 2h, 3.41g silica sol (30%) was added, and after stirring for 1h, 14.83g phosphoric acid (85%) was added dropwise, and after stirring for 1h, a mixed solution was obtained, and the mixed solution was aged at room temperature for 2h and crystallized at 200℃ for 24h. The obtained product was washed by centrifugation with deionized water, filtered, and dried, and then calcined at 650℃ in air atmosphere for 5h to obtain small crystal SAPO-34 molecular sieve D3, and the synthetic yield of the molecular sieve was 54%. The molar ratio of each component material in the mixed solution is: 6R: 0.26SiO2: Al2O3: 0.96P2O5: 13H2O, wherein a / d is 0.46.
[0120] The XRD spectrum of synthetic SAPO-34 molecular sieve D3 is as follows Figure 1 As shown, the microscopic morphology is Figure 8 As shown in the SEM photograph, the SAPO-34 molecular sieve has a cubic morphology and an average particle size of 3.5 μm.
[0121] from Figure 1 It can be seen that the sample prepared in Comparative Example 3 shows characteristic diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, and 25.1±0.1°, indicating that the prepared sample is a SAPO-34 molecular sieve with a CHA topological structure.
[0122] Comparative Example 4
[0123] The SAPO-34 molecular sieve was prepared according to the method of Example 1, only the order of adding the aluminum source and the silicon source was changed, and the other conditions remained unchanged to obtain the molecular sieve D4, the synthesis yield of the molecular sieve was 52%, and the average particle size of the molecular sieve D4 was 25μm. The molecular sieve D4 was subjected to XRD test. The XRD results showed that the molecular sieve D4 not only had the characteristic peak diffraction peaks of SAPO-34 at 2θ=9.5±0.1, 15.9±0.1, 20.5±0.1, 25.1±0.1°, but also had the characteristic peak diffraction peak of SAPO-5 at 2θ=7.36°, indicating that the molecular sieve D4 was not a pure phase SAPO-34 molecular sieve, but contained a SAPO-5 impurity phase. The microscopic morphology of the molecular sieve D4 is as follows: Fig. 9 As shown in the SEM photo of Fig. 9 It can be seen that the molecular sieve D4 contains a SAPO-5 molecular sieve with a prismatic structure.
[0124] Comparative Example 5
[0125] The SAPO-34 molecular sieve was prepared according to the method of Example 1, except that the order of adding the aluminum source and the phosphorus source was changed, and the other conditions remained unchanged to obtain the molecular sieve D5. The synthesis yield of the molecular sieve was 40%, and the average particle size of the molecular sieve D5 was 15 μm. The microscopic morphology of the molecular sieve D5 is shown in FIG. Fig.10 As shown in the SEM photo of Fig.10 It can be seen that the non-cubic block structure in the figure is the amorphous phase, indicating that the molecular sieve D5 is not a pure phase SAPO-34 molecular sieve.
[0126] Test Example 1
[0127] The molecular sieve catalysts prepared in Examples 1-9 and Comparative Examples 1-5 were evaluated in a methanol to olefins reaction using a fixed bed catalytic reaction evaluation device.
[0128] The evaluation conditions are as follows: 0.8 g of the above molecular sieve catalyst samples were weighed and put into the reactor, activated with nitrogen at 500°C for 0.5 h, and then cooled to 450°C. The raw methanol solution was mixed with the carrier gas-nitrogen after passing through the flow metering pump and entered the preheating furnace, where it was vaporized into gas and then entered the reactor for reaction. The nitrogen flow rate was 14 mL / min and the methanol space velocity was 3.50 h -1 The product after the reaction was analyzed online using an Agilent 7890B chromatograph. The catalyst service life was calculated from the time from the start of the reaction to the time when the methanol conversion rate reached 99%. Table 1 lists the specific experimental results of the embodiments and comparative examples.
[0129] Table 1 Evaluation results of methanol conversion to olefins
[0130] <![CDATA[C2H4(%)]]> <![CDATA[C3H6(%)]]> <![CDATA[C2H4+C3H6(%)]]> <![CDATA[C 4+ (%)]]> <![CDATA[C 5+ (%)]]> Lifespan (min) Example 1 49.53 34.84 84.37 8.66 2.62 235 Example 2 49.05 35.07 84.12 9.12 2.75 230 Example 3 49.63 33.77 83.40 8.47 2.94 230 Example 4 49.33 34.59 83.92 8.66 2.85 220 Example 5 49.21 34.47 83.68 9.01 2.31 220 Example 6 49.03 34.29 83.32 8.73 3.27 218 Example 7 48.76 34.00 82.76 9.41 2.95 215 Example 8 48.63 34.55 83.18 8.99 3.00 210 Example 9 49.01 33.98 82.99 9.58 3.06 210 Comparative Example 1 47.08 34.95 82.03 9.62 2.8 135 Comparative Example 2 43.63 38.28 81.91 8.5 1.62 150 Comparative Example 3 47.67 34.41 82.08 9.14 3.35 155 Comparative Example 4 44.52 35.45 79.97 10.80 4.98 130 Comparative Example 5 40.25 33.17 73.42 13.50 6.21 90
[0131] It can be seen from the results in Table 1 that the small-grain SAPO-34 molecular sieve catalyst prepared by the method of the present invention can effectively shorten the diffusion of product molecules in the crystal pores, effectively inhibit the formation of carbon deposits, and extend the catalyst life compared with the SAPO-34 molecular sieve catalyst synthesized by the conventional method.
[0132] Furthermore, the small-grain SAPO-34 molecular sieve prepared by the present invention can extend the life of the catalyst while having high diene (ethylene+propylene) selectivity.
[0133] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing small-grain SAPO-34 molecular sieve, It is characterized in that The method comprises the following steps: (1) mixing an aluminum source, a high-silicon SAPO-34 molecular sieve, a template agent and water and performing pretreatment to obtain an initial gel; (2) mixing the initial gel with a silicon source and a phosphorus source to obtain a mixed solution, and aging, hydrothermally crystallizing, and calcining the mixed solution to obtain the small-grain SAPO-34 molecular sieve; The amount of the aluminum source, the high silicon SAPO-34 molecular sieve, the template, the water, the silicon source and the phosphorus source is such that the molar ratio of the components in the mixed solution is: aR:bSiO 2 :Al 2 O 3 :cP 2 O 5 :dH 2 O, where R is a template, 0.5≤a≤8; 0.1≤b≤1; 0.1≤c≤2.5; 5≤d≤20; 0.3 <a / d<0.6; The pretreatment temperature is 30-80°C, and the pretreatment time is 2-48h.
2. The preparation method according to claim 1, in, The Si / Al ratio of the high-silicon SAPO-34 molecular sieve is 0.4-0.
6.
3. The preparation method according to claim 1 or 2, in, The amount of the aluminum source, the high silicon SAPO-34 molecular sieve, the template, the water, the silicon source and the phosphorus source is such that the molar ratio of the components in the mixed solution is: aR:bSiO 2 :Al 2 O 3 :cP 2 O 5 :dH 2 O, where R is a template, 2≤a≤6; 0.2≤b≤0.5; 0.8≤c≤1.5; 10≤d≤15; 0.4 <a / d<0.5。 4. The preparation method according to claim 1 or 2, in, The aging conditions include: aging time of 2-48h, aging temperature of 30-80°C.
5. The preparation method according to claim 1 or 2, in, The conditions for the hydrothermal crystallization include: a hydrothermal crystallization temperature of 170-210° C. and a hydrothermal crystallization time of 6-40 hours.
6. The preparation method according to claim 1 or 2, in, The calcination conditions include: a calcination temperature of 500-700° C. and a calcination time of 2-12 hours.
7. The preparation method according to claim 1 or 2, in, The phosphorus source is selected from at least one of phosphoric acid, phosphorous acid and phosphorus pentoxide.
8. The preparation method according to claim 1 or 2, in, The aluminum source is selected from at least one of pseudo-boehmite, aluminum sol and aluminum isopropoxide.
9. The preparation method according to claim 1 or 2, in, The silicon source is selected from at least one of silica sol, tetraethyl orthosilicate and active silicon dioxide.
10. The preparation method according to claim 1 or 2, in, The template agent is selected from at least one of triethylamine, diisopropylamine, diethylamine, morpholine, N,N-diisopropylethylamine, cyclohexylamine and n-butylamine.
11. A small-crystal SAPO-34 molecular sieve prepared by the preparation method according to any one of claims 1 to 10.
12. The small-grain SAPO-34 molecular sieve according to claim 11, in, The average particle size of the small-grain SAPO-34 molecular sieve is 0.5-1.5 μm.
13. Use of the small-grain SAPO-34 molecular sieve according to claim 11 or 12 in methanol to olefins.
14. A method for preparing olefins from methanol, It is characterized in that The method comprises: in the presence of a protective gas, methanol and a molecular sieve are contacted and reacted; The molecular sieve is the small-grain SAPO-34 molecular sieve described in claim 11 or 12.
Citation Information
Patent Citations
Method for preparing small granulated SAPO-34 molecular sieve, product prepared through method, and use of product
CN104340986A
Preparation method of small-grain-size SAPO-34 molecular sieve
CN104445266A
Synthetic method of flaky nano-SAPO-34 molecular sieve
CN105585022A
Small-particle-size SAPO-34 molecular sieve as well as preparation method and application thereof
CN112824322A