Coated building panels

By using microporous molecular sieve and acrylic emulsion composition on the building board, the penetration and diffusion of water-based ink on the decorative building board is solved, the image resolution and color intensity are improved, and high-quality Water-based ink inkjet printing effect.

CN116209724BActive Publication Date: 2024-11-12SUDARSHAN SWISS HOLDINGS LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180057137.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-06
Filing Date
2021-07-14
Publication Date
2024-11-12
Estimated Expiration
2041-07-14

AI Technical Summary

Technical Problem

Water-based ink is prone to permeation or diffusion in inkjet printing on decorative building boards, resulting in poor image quality, poor resolution and color intensity, and difficult to stabilize and fix.

Method used

采用包含微孔分子筛的水性涂料组合物,通过在建筑板表面施加丙烯酸乳液和分子筛的组合物,并在特定温度下固化,形成颜色成像层以提高墨的固着性和图像稳定性。

Benefits of technology

The image resolution and color intensity of water-based inkjet printing is significantly improved, the color leakage is reduced, the image stability and friction resistance are enhanced, the penetration of water-based ink is avoided, and high-quality color imaging is achieved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to a coated building board comprising a color imaging layer for water-based inks and a method of making the coated building board. The present invention particularly relates to a coated building board wherein the color imaging layer comprises a molecular sieve, in particular a microporous zeolite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coated building board comprising a color imaging layer for water-based inks and a method of making the coated building board. The present invention particularly relates to a coated building board wherein the color imaging layer comprises a molecular sieve. Background Art

[0002] Color patterns can be applied to various types of decorative building boards by, for example, inkjet printing, which allows efficient production and personalized design. Compared with solvent-based inks and UV inks, water-based inks are more popular because pigments with higher weather resistance can be applied, which is suitable for exterior wall applications. Another important advantage is that water-based inks are more environmentally friendly.

[0003] On the other hand, performing aqueous inkjet printing is challenging because water-based inks are difficult to cure compared to solvent inks or UV inks. As a result, water-based inks tend to penetrate into the base material (especially if the base material is porous) or spread on the surface (if the base material is non-porous). This results in poor image quality.

[0004] In order to improve the color intensity of images printed with water-based ink on decorative building boards, JP2007154433 proposes an ink receiving layer fixed on the surface of the building board. The ink receiving layer is a water-based coating containing an inert pigment and a hygroscopic resin. JP 2007167826 describes the use of such a coating composition to reduce ink consumption in inkjet printing. In order to inhibit the penetration of ink into the ink receiving layer and stably fix the ink, an ink receiving layer containing polysiloxane is proposed in JP 2015051549.

[0005] JP 2008273055 discloses a coating composition for an ink receiving layer, which contains 20 to 80 wt % of a mica filler based on the solid content of the coating composition to enhance the durability of the coating.

[0006] JP 2008063832 provides a decorative building board that enhances the fixation of ink to an ink receiving layer and prevents the strength of the layer from decreasing. To achieve the desired effect, the ink receiving layer contains a filler having a high aspect ratio of 3 to 70 that can be finely divided on the surface of the layer.

[0007] The problem to be solved by the present invention is to provide a building board which can be used as a base material for printing high-quality images with water-based inks. In particular, the resolution of the printed image, the color intensity and the stability of the image are to be improved. To achieve the object of the present invention, the penetration of the water-based ink into the building board should be reduced to avoid low color intensity, and bleeding should be avoided to achieve improved resolution of the printed pattern. Summary of the invention

[0008] The problem is solved by a color imaging layer (ink receiving layer) comprising a molecular sieve.

[0009] Molecular sieves are porous materials with relatively uniform pore sizes. The pore size of a molecular sieve is similar to the size of a small molecule, so unlike small molecules such as water, large molecules cannot be adsorbed. The diameter of a molecular sieve is measured in angstroms. Or nanometers (nm) are used as units of measurement. Molecular sieves are classified into those with pore sizes less than 2nm. Microporous materials with pore sizes between 2-50nm Mesoporous materials with pore sizes greater than 50 nm Macroporous materials. Pore size greater than 200nm Macroporous materials are not considered to be molecular sieves in the sense of the present invention.

[0010] The coated building board of the present invention is obtained from an aqueous coating composition comprising an acrylic emulsion and a molecular sieve, and the aqueous coating composition can be cured on the surface of the building board.

[0011] Thus, one embodiment of the present invention is a method of making a coated building panel comprising a color imaging layer, wherein the method comprises:

[0012] a) applying an aqueous coating composition to at least a portion of a surface of a building panel, the coating composition comprising:

[0013] i) 20 to 80 wt % of an acrylic polymer emulsion, and

[0014] ii) 0.2 wt % to 20 wt % of the coating composition of a molecular sieve, and

[0015] b) curing the coating composition.

[0016] To achieve the intended effect of the present invention, microporous molecular sieves are preferably used. Preferred molecular sieves have a narrow pore size distribution, wherein at least 90% of the pores of the molecular sieve have a pore size between 0.1 nm and 2 nm, more preferably between 0.2 nm and 0.8 nm.

[0017] The microporous molecular sieve may be selected, for example, from aluminosilicate minerals (zeolites), phosphorus-modified small pore zeolites, porous glasses, activated carbons, and small pore clays such as montmorillonite.

[0018] Preferred molecular sieves are capable of adsorbing molecules having an effective diameter of 0.5 nm or less, such as water. Useful molecular sieves are capable of adsorbing at least 5 wt% water at 20°C, more advantageously greater than 10 wt% water, compared to the weight of the molecular sieve.

[0019] Preferred microporous molecular sieves are from the group of zeolites. Particularly preferred are or Zeolite.

[0020] Suitable zeolites have the general formula (I):

[0021] Mn + x / n ·[(AlO2) - x ·(SiO2) y ]·z H2O (I)

[0022] in

[0023] n is 1, 2, 3 or 4, preferably n is 1 or 2;

[0024] M is selected from monovalent, divalent, trivalent or tetravalent metals or mixtures thereof, preferably M is selected from alkali metals, alkaline earth metals and mixtures thereof, wherein metal potassium, sodium, magnesium and calcium are most preferred;

[0025] x is between 1 and 10, preferably between 1 and 3, and

[0026] The x / y ratio of the zeolite of formula (I) is between 1 and 5, more preferably between 1 and 3 and most preferably the ratio is about 2, ie between 1.8 and 2.2.

[0027] The water content of zeolite can vary within a wide range. For example, water can be removed from zeolite by heating without destroying the zeolite structure. Vice versa, zeolite can absorb water until the capacity of the compound is exhausted. Dry zeolites of preferred zeolite types (x and x / y in the range of 1 to 3) are, for example, capable of adsorbing up to 30% by weight of water compared to the zeolite weight. The water content z of the zeolite of formula (I) is typically in the range of 0 to 50, preferably between 1 to 30. For preferred zeolites, wherein x is in the range of 1 to 3 and the x / y ratio is in the range of 1 to 3, z is typically less than 10.

[0028] The most preferred zeolite molecular sieve is or Zeolite sieve.

[0029] Typical Sieve has the chemical formula:

[0030] x'K2O·x”Na2O·Al2O3·y SiO2·z H2O

[0031] in

[0032] x' and x" are in the range of 0.3 to 0.7, and x'+x" is 1;

[0033] y is in the range of 1.8 to 2.2, preferably y is 2, and

[0034] z is less than 8, preferably z is in the range of 3 to 6, typically 4.5.

[0035] Typical Sieve has the chemical formula:

[0036] Na2O·Al2O3·y SiO2·z H2O

[0037] in

[0038] y is in the range of 1.8 to 2.2, preferably y is 2, and

[0039] z is less than 8, preferably z is in the range of 3 to 6, typically 4.5.

[0040] Typical Sieve has the chemical formula:

[0041] x'CaO·x”Na2O·Al2O3·y SiO2·z H2O

[0042] in

[0043] x' is in the range of 0.6 to 0.8,

[0044] x" is in the range of 0.2 to 0.4, and

[0045] x'+x" is 1;

[0046] y is in the range of 1.8 to 2.2, preferably y is 2, and

[0047] z is less than 8, preferably z is in the range of 3 to 6, typically 4.5.

[0048] include and A wide variety of microporous molecular sieves, including zeolites, are commercially available. However, they can be prepared as follows Sieve: Aqueous solutions of sodium silicate and sodium aluminate were mixed at 80° C. The sieve was then activated by baking at 400° C. Sieve and The sieve can be The sieve was started by exchanging the sodium cations for potassium (for sieve) or exchange sodium cations for calcium (for sieve) to prepare.

[0049] Medium pore molecular sieves are, for example, silicon dioxide. Examples of large pore molecular sieves are those with pore sizes of 200- of porous silica compounds.

[0050] The pore size of a molecular sieve depends on the size of the crystal lattice of the material itself, which is mainly determined by the size of the cations. The structures of a wide range of zeolites, including the size of the channels (pores), are summarized in "Atlas of Zeolite Framework Types" (Baerlocher et al., Elsevier, Sixth Revised Edition, 2007).

[0051] Preferred molecular sieves are capable of adsorbing molecules having an effective diameter of 0.5 nm or less, such as water. Useful molecular sieves are capable of adsorbing at least 5 wt% water, more advantageously greater than 10 wt% water, compared to the weight of the molecular sieve.

[0052] The molecular sieve is preferably applied to the aqueous coating composition in powder form. Preferred powders have an average particle diameter in the range of 0.1 μm to 250 μm, preferably an average diameter between 1 μm and 50 μm. At least 80%, in particular at least 90%, of the particles should have an average diameter within this range.

[0053] The size distribution of molecular sieve particles can be determined by laser diffraction analysis. The average diameter can be determined by laser scattering, for example by using a Horiba LA940 or Master sizer 3000 from Malvern using the "Mie scattering theory" evaluation to determine. In the case of particles having axes of different lengths, such as particles with an elliptical or disc shape, the largest axis determines the average diameter. The particles of the present invention preferably have a narrow particle size distribution with a Gaussian shape. Preferably, the standard deviation of the particle size distribution is between 10% and 120% of the average diameter. More preferably, the standard deviation is between 20% and 90%.

[0054] The coating composition further comprises an acrylic emulsion. The acrylic emulsion comprises an acrylic polymer obtained by free radical polymerization of an acrylic monomer composition, wherein the acrylic monomer is selected from the group consisting of acrylates, methacrylates, alkyl acrylates, alkyl methacrylates, hydroxyalkyl acrylates, hydroxyalkyl methacrylates, epoxyalkyl acrylates, epoxyalkyl methacrylates, acrylonitrile, methacrylonitrile, acrylamide, methacrylamide, acrylic acid, and mixtures thereof, and optionally ethylenically unsaturated comonomers.

[0055] Preferred acrylic polymers are derived from acrylates, methacrylates, (C1-C4)-alkyl acrylates, (C1-C4)-alkyl methacrylates, acrylic acid and mixtures thereof and optionally ethylenically unsaturated comonomers.

[0056] Preferred comonomers are selected from (C1-C6)-olefins, in particular ethylene, propylene and butene, and styrene.

[0057] Acrylic polymer emulsions also include emulsions of acrylic silicone resins.

[0058] The acrylic monomer composition preferably comprises at least 50 weight percent acrylic monomers and less than 50 weight percent ethylenically unsaturated comonomers.

[0059] The content of the acrylic polymer in the acrylic emulsion is 5-75% by weight, preferably 10-70% by weight, and particularly preferably 20-60% by weight.

[0060] The water content of the acrylic polymer emulsion is 25-75% by weight, preferably 30-60% by weight.

[0061] The aqueous coating composition comprising an acrylic polymer emulsion and a molecular sieve particularly comprises 1 wt % to 10 wt % of the molecular sieve. Based on the total weight of the aqueous coating composition, the amount of the acrylic polymer emulsion is preferably in the range of 25 wt % to 60 wt %, particularly in the range of 30 to 55 wt %.

[0062] The weight ratio of the micromesh to the acrylic polymer in the aqueous coating composition is preferably 1:1 to 1:100. A more preferred ratio is 1:1.5 to 1:20, and a most preferred ratio is in the range of 1:2 to 1:10.

[0063] The aqueous coating composition may contain optional additives. Examples of useful additives are dispersants, wetting agents, thickeners, defoamers, fillers, film formers, matting agents, neutralizers or biocides. The additives may be applied to the acrylic polymer emulsion or to the aqueous coating composition comprising the emulsion.

[0064] Common additives include wetting agents or dispersants, such as sodium, potassium or ammonium polyphosphates, alkali metal or ammonium salts of polyacrylic acid and polymaleic acid, styrene maleic anhydride copolymers, polyphosphonates, amino alcohols such as 2-amino-2-methylpropanol. The amount of dispersants or wetting agents is preferably up to 2% by weight based on the total weight of the aqueous coating composition.

[0065] Typically the acrylic polymer of the acrylic polymer emulsion is self-emulsifiable. Therefore, the amount of additional dispersant can be low. The content of dispersant in the aqueous coating composition is less than 5 wt %, preferably in the range of 0 to 1 wt %, based on the total weight of the aqueous coating composition.

[0066] Antifoam additives are, for example, fatty acid alkyl ester alkoxylates, silicone oils, organopolysiloxanes such as polydimethylsiloxane, polyether-modified polysiloxanes, silanized silicas, paraffins (including paraffin oils), waxes, polyethers (such as polyethylene glycol, polypropylene glycol or EO / PO copolymers), and mixtures thereof.

[0067] The defoamer is typically used in an amount of less than 5% by weight, in particular in the range of 0 to 2% by weight, based on the total amount of the aqueous coating composition.

[0068] The matting agent may be present in the aqueous coating composition in an amount of 0 to 15 wt %, based on the total weight of the coating composition. The preferred matting agent content is 1 to 10 wt %. Suitable matting agents are silica and waxes.

[0069] Thickeners which can be used in aqueous coating compositions are, for example, cellulose derivatives, such as methylcellulose, hydroxyethylcellulose and carboxymethylcellulose, and also casein, gum arabic, starch, sodium alginate, polyvinyl alcohol, polyvinyl pyrrolidone, styrene / maleic anhydride polymers, polyether polyurethanes (which may be hydrophilically modified), hydrophobically modified acrylic copolymers (HASE), sodium polyacrylate, silicones and polyether polyols.

[0070] Water-soluble copolymers based on acrylic acid and (meth)acrylic acid, such as acrylic acid / acrylamide and (meth)acrylic acid / acrylate copolymers, also have thickening properties.

[0071] Inorganic thickeners such as bentonite may also be used.

[0072] Thickeners from the group of acrylic polymers and polyurethanes are particularly advantageously used.

[0073] The amount of thickener is less than 10 wt%, preferably less than 5 wt%, based on the total weight of the coating composition.

[0074] Suitable film formers are for example polyvinyl pyrrolidone, glycol ether or glycol ester or its combination.The example of glycol ether is ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, ethylene glycol monophenyl ether, ethylene glycol monohexyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol ethylene glycol mono-n-butyl ether, diethylene glycol mono-n-hexyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monohexyl ether, polyoxyethylene glycol ether, polypropylene glycol ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether and ethylene glycol dibutyl ether.Diol ester is for example ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate and propylene glycol methyl ether acetate.

[0075] The content of the film-forming additive is generally less than 10% by weight based on the total amount of the aqueous coating composition, preferably in an amount within the range of 0.5 to 5% by weight.

[0076] Fillers that can be used are known to those skilled in the art. Preferred fillers are silicates, such as kaolin, talc, mica, magnesite, alkaline earth metal carbonates (e.g. calcite, chalk, dolomite), alkaline earth metal sulfates such as calcium sulfate, and silicon dioxide. Fillers can be used as individual components or as filler mixtures. In general, finely divided fillers are preferred.

[0077] The waterborne coating composition optionally comprises one or more cosolvents. Cosolvents can be a part of the additive composition. A small amount of cosolvents can be added to improve the solubility of the components of the waterborne coating composition. Based on the gross weight of the coating composition, the amount of cosolvent should be less than 10 weight %. Preferably, the cosolvent content is less than 5 weight %.

[0078] Suitable are water-miscible cosolvents, for example methanol, ethanol, propanol, butanol, benzyl alcohol, ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, glycerol, polyethylene glycol, polypropylene glycol, and monomethyl or dimethyl ethers of ethylene glycol or propylene glycol.

[0079] For some applications, the pH of the aqueous coating composition needs to be adjusted. To adjust the pH, common neutralizers can be used. Examples of neutralizers are sodium hydroxide, potassium hydroxide or amine derivatives. For most applications, a pH in the range of 7 to 11 is desired. The neutralizer is added to the coating composition until the desired pH is reached.

[0080] The waterborne coating composition may also include a pigment. The pigment may be selected from an inorganic pigment or an organic pigment. The pigment that may be used is all pigments for emulsion paints known to those skilled in the art. Preferred pigments are, for example, titanium dioxide (preferably in the form of rutile), barium sulfate, zinc oxide, zinc sulfide, basic lead carbonate, antimony trioxide, and lithopone (zinc sulfide and barium sulfate). However, the waterborne formulation may also include a colored pigment, such as iron oxide, carbon black, graphite, luminescent pigment, zinc yellow, zinc green, ultramarine, manganese black, antimony black, or manganese violet. Organic pigments are, for example, azo dyes, quinacridones, phthalocyanines, isoindolinones, sepia pigments, gamboge, indigo, anthraquinones and indigo dyes and dioxazines, and metal complex pigments.

[0081] The most preferred pigments are titanium dioxide, zinc oxide, barium sulfate and lithopone.

[0082] Pigments can be added to the aqueous coating composition in an amount of up to 30 wt %, based on the total weight of the aqueous coating composition. Light pigments can typically be added in larger amounts, while dark pigments are typically added in lower amounts of up to 15 wt %.

[0083] Preferably, light-colored pigments, such as titanium dioxide, zinc oxide, barium sulfate and lithopone, are added to the coating composition in an amount of 5 to 25% by weight.

[0084] The pigment may be mixed with an inert pigment, such as silicon dioxide, barium carbonate, calcium carbonate, aluminum oxide, aluminum hydroxide, diatomaceous earth, and the like.

[0085] In addition to the acrylic polymer, the coating composition may optionally contain another polymer. Suitable optional polymers may be selected from hygroscopic polymers. For example, polyvinyl acetate, polyvinyl alcohol and polyurethane may be optionally added.

[0086] Based on the total weight of the aqueous coating composition, the optional polymer can be added in an amount of up to 50% by weight. The content of the optional polymer in the coating composition is preferably 0 to 30% by weight, in particular 5 to 25% by weight. Particularly preferred are coating compositions that do not contain the optional polymer or have a content of the optional polymer of less than 5% by weight.

[0087] The molecular sieve can be added to the acrylic polymer emulsion to obtain an aqueous coating composition. The molecular sieve can be simply incorporated into the acrylic polymer emulsion by stirring until the molecular sieve is fully dispersed. Additives and pigments can be added under stirring, usually stepwise.

[0088] In addition to the water already present in the acrylic polymer emulsion, additional water can be added to the aqueous coating composition if appropriate. However, the total content of water in the coating composition should be less than 80% by weight. Preferably, the total water content is in the range of 25 to 65% by weight.

[0089] The aqueous coating composition can be applied to the surface of the building board by a spraying device such as a spray gun. Alternatively, the coating composition can be brushed onto the surface or applied with a scraper.

[0090] Typically, the waterborne coating composition is applied at a rate of 10 g / m 2 Up to 300g / m 2 , preferably at 20g / m 2 Up to 200g / m 2 within the range.

[0091] The aqueous coating composition applied to the building board is then cured to obtain a color imaging layer on the surface of the building board. Curing can be achieved by drying the coating at a temperature between 80°C and 300°C for 1 minute to 1 hour. If the resulting color imaging layer is able to capture the water-based ink, the coating is sufficiently dry. The coated building board can be dried in an oven. Preferably, the drying is performed at a temperature between 150°C and 250°C for 2 to 150 minutes.

[0092] The thickness of the color imaging layer on the building board is generally between 5 μm and 500 μm, preferably between 10 μm and 200 μm.

[0093] A variety of building materials can be used as building boards, as long as the color imaging layer can be sufficiently fixed on the surface. For example, cement boards, gypsum boards, ceramic boards, metal boards, wood boards or polymer resin boards are suitable building boards. Preferably, building boards made of cement or gypsum are used. The adhesion of the color imaging layer to these boards is excellent. Also suitable are fiber-reinforced building boards, in particular cement boards containing glass fibers or polymer fibers.

[0094] The coated building board preferably comprises a sealing layer or a primer layer. The sealing layer or primer layer can be applied on the surface of the building board. Thus, the surface of the building board on which the aqueous coating composition is applied is formed by such a layer. More preferably, the primer layer is applied to provide a background color, especially if a non-pigmented color imaging layer is applied afterwards. For example, a building board comprising a sealing layer and a white primer layer is particularly useful. Sealing compositions and primer compositions particularly for cement or gypsum boards are known in the art.

[0095] Conventional primer compositions include aqueous emulsions of polyvinyl acetate, copolymers of vinyl acetate and ethylene, copolymers of acrylates and styrene, and aqueous solutions of polyvinyl alcohol, for example. Typical sealants are water-based or solvent-based acrylic resins, epoxy resin / polyurethane systems, silanes, silicates, siliconates, siloxanes, and the like.

[0096] Another embodiment of the present invention is a coated building panel comprising a color imaging layer of the cured coating composition as described above.

[0097] The color imaging layer applied to at least a portion of the surface of the coated building board of the present invention preferably comprises, after curing, 30 to 95 weight percent acrylic polymer and 0.5 to 50 weight percent molecular sieve layer.

[0098] Compared with the water content of the aqueous coating composition, the water content of the color imaging layer is significantly reduced. The water content of the color imaging layer is usually less than 10% by weight of the molecular sieve weight, preferably less than 5% by weight, and particularly preferably less than 3% by weight. Typically, the water content is in the range of 0.1 to 2% by weight.

[0099] The weight ratio of molecular sieve to acrylic polymer in the color imaging layer of the coated building board is preferably from 1:1 to 1:100. A more preferred ratio is from 1:1.5 to 1:20, and a most preferred ratio is in the range of 1:2 to 1:10.

[0100] Preferred coated building panels of the present invention comprise a color imaging layer comprising

[0101] a) 30 to 80% by weight of an acrylic acid polymer,

[0102] b) 5 to 40% by weight of molecular sieves,

[0103] c) optionally 0.2 to 2% by weight of a defoamer,

[0104] d) optionally 0.2 to 4% by weight of a dispersant,

[0105] e) optionally 0 to 15% by weight of a matting agent,

[0106] f) optionally 3 to 10% by weight of a film former,

[0107] g) optionally 0.5 to 8% by weight of a thickener,

[0108] h) optionally up to 0.5% by weight of a biocide, and

[0109] i) Optionally up to 0.5% by weight of a neutralizing agent.

[0110] Another preferred embodiment of the coated building panel includes a color imaging layer comprising

[0111] a) 30 to 75% by weight of an acrylic acid polymer,

[0112] b) 5 to 35% by weight of molecular sieves,

[0113] c) optionally 0.2 to 2% by weight of a defoamer,

[0114] d) optionally 0.2 to 4% by weight of a dispersant,

[0115] e) optionally 0 to 15% by weight of a matting agent,

[0116] f) optionally 3 to 10% by weight of a film former,

[0117] g) optionally 0.5 to 8% by weight of a thickener,

[0118] h) optionally up to 0.5% by weight of a biocide,

[0119] i) optionally up to 0.5% by weight of a neutralizing agent, and

[0120] j) 5 to 30% by weight of pigments.

[0121] Preferred defoamers, dispersants, matting agents, film formers, thickeners and neutralizers are as described above.

[0122] The coated building board is particularly suitable for printing a colored pattern or image on the color imaging layer using a water-based ink. The water-based ink can be printed directly onto the color imaging layer, for example by inkjet printing. The printed pattern can be easily personalized. The coated building board is suitable for DIY (do it yourself) printing.

[0123] If water-based ink is applied to the color imaging layer, the ink is quickly fixed and bleeding is significantly reduced. The resolution of the printed pattern or image is improved. In addition, the rapid penetration of the water-based ink into the color imaging layer is avoided, which helps to improve the color intensity.

[0124] Without being bound by any theory, the desired effect is achieved by the molecular sieve accelerating water absorption from the water-based ink while significantly retarding the penetration of colorants and pigments provided as components of the water-based ink into the color imaging layer. This results in low bleed and high color intensity.

[0125] The color imaging layer is particularly suitable for use with water-based inks having a water content of 40-70% by weight and a pigment content of 3-20% by weight. Typical water-based inks also contain up to 40% by weight of humectants such as glycerol, propylene glycol, etc., up to 2% by weight of surfactants such as polyoxyethylene alkyl ethers, and pH adjusters. Optionally, the water-based ink may contain up to 10% by weight of an acrylic resin.

[0126] Therefore, another embodiment of the present invention is the use of a building board comprising a color imaging layer as described herein as a base material for inkjet printing with water-based inks. DETAILED DESCRIPTION

[0127] Embodiment 1 (E1):

[0128] 40 parts by weight of deionized water, 45 parts by weight of acrylic emulsion (Mowilith DN 7070, Archroma Co. Ltd.), 0.3 parts by weight of defoamer (BYK-022, BYK Additives & Instruments), 0.15 parts by weight of dispersant (BYK-190, BYK Additives & Instruments), 3.5 parts by weight of silica (SYLOID W 300, WR Grace & Co.), 2.7 parts by weight of wax powder (Ceridust 8090TP, Clariant Chemicals Ltd) were mixed with a disperser at a shear rate of 1000 rpm for 30 minutes, and then 3 parts by weight of film former (DOWANOL TMDPnB, DowChemical), 0.5 parts by weight of thickener (Mowiplus TK-582, Archroma Co. Ltd), 0.075 parts by weight of biocide (Acticide LA 0614, Thor Chemie), and gradually add about 0.075 parts by weight of neutralizer 2-amino-2-methyl-1-propanol (AMP 95, Dow Chemical) to adjust the pH to 8-10. The mixture was dispersed for 60 minutes at a shear rate of 1500 rpm by a disperser. Finally, 4.7 parts by weight of molecular sieve (SYLOSIV A 3, WR Grace & Co.) were blended into the mixture at a shear rate of 1500 rpm for 30 minutes until fully dispersed to form a coating composition.

[0129] The coating composition was mixed at 80 g / m 3 The amount of the coating was sprayed onto the cement fiber board and cured in an oven at 200° C. for 3 minutes to form a color imaging layer. The cement fiber board was pre-treated with a seal coat and a white primer coat.

[0130] Embodiment 2 (E2):

[0131] 30 parts by weight of deionized water, 40 parts by weight of acrylic emulsion (Neocryl XK-87, DSM NeoResin), 0.25 parts by weight of defoamer (BYK-028, BYK Additives & Instruments), 0.13 parts by weight of dispersant (BYK-190, BYK Additives & Instruments), 3 parts by weight of SYLOID W 300 (WR Grace & Co.) and 2.2 parts by weight of ACEMATT TS100 (Evonik) were mixed by a disperser at a shear rate of 1000 rpm for 30 minutes, and then 15 parts by weight of titanium dioxide (Colanyl White TQ-CN, Clariant Chemicals Ltd), 2.5 parts by weight of film former (DOWANOL TMDPnB, Dow Chemical), 0.4 parts by weight of a mixed thickener (Mowiplus TK-582, Archroma Co. Ltd), 0.06 parts by weight of a biocide (Acticide LA 0614, Thor Chemie), and about 0.06 parts by weight of a neutralizer 2-amino-2-methyl-1-propanol (AMP 95, Dow Chemical) are gradually added to adjust the pH to 8-10. The mixture is dispersed for 60 minutes at a shear rate of 1500 rpm by a disperser. Finally, 6.4 parts by weight of a molecular sieve (SYLOSIV A3, WR Grace & Co.) are blended into the mixture at a shear rate of 1500 rpm for 30 minutes until fully dispersed to form a coating composition.

[0132] The coating composition was mixed at 140 g / m 3 The amount of the coating was sprayed onto the cement fiber board and cured in an oven at 200° C. for 3 minutes to form a color imaging layer. The cement fiber board was pre-treated with a seal coat.

[0133] Embodiment 3 (E3):

[0134] 30 parts by weight of deionized water, 53.1 parts by weight of acrylic emulsion (Neocryl XK-87, DSM NeoResin), 0.34 parts by weight of defoamer (BYK-022, BYK Additives & Instruments), 0.17 parts by weight of dispersant (Dispersogen LFH, Clariant Chemicals Ltd), 3 parts by weight of SYLOID W 300 from WR Grace & Co., 1.3 parts by weight of ACEMATT TS100 (Evonik) and 2.7 parts by weight of Ceridust 8090TP (Clariant Chemicals Ltd) were mixed by a disperser at a shear rate of 1000 rpm for 30 minutes, and then 4 parts by weight of film former (Texanol, Eastman Chemical), 0.6 parts by weight of thickener (Acrysol ASE-60, Dow Chemical), 0.24 parts by weight of biocide (Acticide LA 0614, Thor Chemie), and gradually add about 0.15 weight parts of neutralizing agent triethanolamine to adjust the pH to 8-10. The mixture is dispersed for 60 minutes at a shear rate of 1500 rpm by a disperser. Finally, 4.4 weight parts of molecular sieves (SYLOSIV A 3, WR Grace & Co.) are blended into the mixture at a shear rate of 1500 rpm for 30 minutes until fully dispersed to generate a coating composition.

[0135] The coating composition was coated at 100 g / m 3 The amount of the coating was sprayed onto the gypsum foam board and cured in an oven at 200°C for 3 minutes to form a color imaging layer. The cement fiber board was pre-treated with a seal coat and a white primer.

[0136] Embodiment 4 (E4):

[0137] 35 parts by weight of deionized water, 47 parts by weight of acrylic emulsion (Mowilith DN 7070, Archroma Co. Ltd.), 0.3 parts by weight of defoamer (BYK-022, BYK Additives & Instruments), 0.15 parts by weight of dispersant (BYK-190, BYK Additives & Instruments), 5.5 parts by weight of silica (SYLOID W 300, WR Grace & Co.) were mixed by a disperser at a shear rate of 1000 rpm for 30 minutes, and then 3 parts by weight of film former (DOWANOL TMDPnB, Dow Chemical), 0.5 parts by weight of thickener (Mowiplus TK-582, Archroma Co. Ltd), 0.075 parts by weight of biocide (Acticide LA 0614, from Thor Chemie), and gradually add about 0.075 parts by weight of neutralizer 2-amino-2-methyl-1-propanol (AMP 95, Dow Chemical) to adjust the pH to 8-10. The mixture was dispersed for 60 minutes at a shear rate of 1500 rpm by a disperser. Finally, 8.4 parts by weight of molecular sieve (SYLOSIV A 3, WR Grace & Co.) were blended into the mixture at a shear rate of 1500 rpm for 30 minutes until fully dispersed to form a coating composition.

[0138] The coating composition was applied at 20 g / m 3 The amount of the coating was sprayed onto the aluminum composite panel and cured in an oven at 150°C for 10 minutes to form a color imaging layer. The cement fiberboard was pre-treated with a seal coat and a white primer.

[0139] Comparative Example 1 (CE1):

[0140] The cement fiberboard was pre-treated with a seal coat and a white primer, but no color imaging layer was applied.

[0141] Comparative Example 2 (CE2):

[0142] Example 1 was repeated in the absence of molecular sieves to produce a coating composition without molecular sieves. The resulting coating composition was heated at 80 g / m 3 The amount of the coating was sprayed onto the cement fiber board and cured in an oven at 200° C. for 3 minutes to form a color imaging layer. The cement fiber board was pretreated with a seal coat and a white primer as described in CE1.

[0143] Comparative Example 3 (CE3):

[0144] Example 1 was repeated by replacing the molecular sieves with the same amount of bentonite.

[0145] Comparative Example 4 (CE4):

[0146] Commercially available decorative acrylic paint was applied at 80 g / m 3 The amount of the coating was sprayed onto the cement fiber board and cured in an oven at 200°C for 3 minutes to form a color imaging layer. The cement fiber board was pre-treated with a seal coat and a white primer.

[0147] Performance evaluation:

[0148] The obtained building board is arranged under an inkjet device equipped with four colors of water-based ink (i.e., cyan, magenta, yellow, and black). The ejection and suspension of the four inks from the nozzles are respectively controlled by a control unit. Inkjet printing is performed by printing a pre-designed image directly on the building board. The building board is then dried in an oven at a temperature of 200° C. for 3 minutes to cure the imaging layer. Preferably, a transparent top coating is sprayed on the cured imaging layer for protection. The obtained image is visually evaluated. The evaluation criteria are as follows:

[0149] * Color intensity, from 1 (very low) to 5 (high)

[0150] * Resolution, from 1 (very blurry and dim, image difficult to discern) to 5 (image clean and sharp)

[0151] * Image stability, from 1 (may become blurry due to finger rubbing) to 5 (image is stable against rubbing or scratching)

[0152] Color Intensity Resolution Image stabilization E1 4 5 5 E2 4 5 4 E3 3 5 5 E4 5 4 2 CE1 1 2 5 CE2 4 2 3 CE3 4 3 3 CE4 3 1 2

[0153] By magnifying the image 60 times, the appearance of the ink dots can be evaluated.

[0154] In CE1, when no imaging layer was applied, the ink dots obtained were very small and light with large gaps. The ink dots were adsorbed by the porous base material, resulting in low color intensity and low resolution. In CE2 and CE4, a curing coating without molecular sieves was applied. The penetration of ink dots into the coating was avoided, thereby significantly improving the color intensity. However, since water-based inks are difficult to cure, the ink dots merge with each other and become irregular, resulting in blurred images. The ink dots obtained in E1-E4 were clear, dense granular, and no bleeding was observed. The images on the building boards containing the color imaging layers according to the present invention (E1-E4) were much clearer than the images on the building boards of comparative examples CE1-CE4. The molecular sieve further increases the fixation of the ink dots, as well as the stability of the image against friction and scratching.

Claims

1. A method for preparing a coated building panel comprising a color imaging layer, the method comprising at least a) applying an aqueous coating composition to at least a portion of the surface of the building board, the composition comprising i) from 20% to 80% by weight of the coating composition of an acrylic polymer emulsion, and ii) 0.2% to 20% by weight of the coating composition of a molecular sieve, and b) curing the coating composition, wherein the molecular sieve is a microporous molecular sieve, and wherein at least 90% of the pores of the molecular sieve have a pore size between 0.1 nm and 2 nm.

2. The method of claim 1, wherein the molecular sieve is selected from zeolites.

3. The method of claim 1, wherein the molecular sieve is a 3Å, 4Å or 5Å zeolite.

4. The method according to claim 1 or 2, wherein the acrylic polymer emulsion comprises an acrylic polymer obtained by free radical polymerization of an acrylic monomer composition, wherein the acrylic monomer composition comprises acrylic monomers and optionally ethylenically unsaturated comonomers, and the acrylic monomers are selected from the group consisting of acrylates, methacrylates, alkyl acrylates, alkyl methacrylates, hydroxyalkyl acrylates, hydroxyalkyl methacrylates, epoxyalkyl acrylates, epoxyalkyl methacrylates, acrylonitrile, methacrylonitrile, acrylamide, methacrylamide, acrylic acid, and mixtures thereof.

5. The method of claim 4, wherein the acrylic monomer composition comprises at least 50 weight percent acrylic monomers and less than 50 weight percent ethylenically unsaturated comonomers.

6. The method according to claim 1 or 2, wherein the acrylic polymer emulsion has a water content of 25 to 75 wt%.

7. The method according to claim 1 or 2, wherein the aqueous coating composition comprises a film former selected from glycol ethers or glycol esters or a combination thereof.

8. The method of claim 1 or 2, wherein the aqueous coating composition comprises up to 50% by weight of a polymer selected from the group consisting of polyvinyl acetate, polyvinyl alcohol and polyurethane.

9. The method according to claim 1 or 2, wherein the aqueous coating composition comprises a dispersant, a thickener, a filler, a defoamer, a neutralizer, a biocide, a matting agent and / or a pigment.

10. A coated building board comprising a color imaging layer of the cured coating composition of any one of claims 1 to 9 on at least a portion of the surface of the building board.

11. A coated building panel comprising a color imaging layer on at least a portion of its surface, wherein the color imaging layer comprises from 30% to 95% by weight of the layer of an acrylic polymer and from 0.5% to 50% by weight of the layer of a molecular sieve, wherein the molecular sieve is a microporous molecular sieve, and wherein at least 90% of the pores of the molecular sieve have a pore size between 0.1 nm and 2 nm.

12. The coated building panel of claim 11 wherein the weight ratio of the molecular sieve to the acrylic polymer in the color imaging layer is from 1:1 to 1:

20.

13. A coated building panel according to claim 11 or 12, wherein the molecular sieve is a zeolite.

14. The coated building panel of claim 11 or 12, wherein the molecular sieve is a 3Å, 4Å, 5Å zeolite or a mixture thereof.

15. The coated building board according to claim 11 or 12, wherein the building board is a cement board, a gypsum board, a ceramic board, a metal board, a wood board or a polymer resin board.

16. Use of a building board according to any one of claims 10 to 15 as a base material for inkjet printing with water-based inks.

Citation Information

Patent Citations

  • Decorative building plate and its manufacturing method

    JP2007154433A

  • Decorative construction plate

    JP2007167826A

  • Decorative building board

    JP2008063832A

  • Coating composition for ink receiving layer and decorative building board

    JP2008273055A

  • Coated plate

    JP2015051549A