A 500MPa multi-wire submerged arc welding wire and welding wire capable of welding at 50-150kJcm heat input

By optimizing the chemical composition and flux of multi-wire submerged arc welding electrodes and welding wires, the problem of insufficient weld metal strength and low-temperature toughness in high heat input welding was solved, achieving high-efficiency welding and meeting the welding needs of large steel structures such as bridges.

CN116252067BActive Publication Date: 2024-11-22YANSHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310017320.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-06
Publication Date
2024-11-22
Estimated Expiration
2043-01-06

AI Technical Summary

Technical Problem

Existing welding wires have insufficient weld metal strength and low-temperature toughness in high-heat-input welding, and low welding efficiency, making it difficult to meet the high-efficiency welding requirements of large steel structures such as bridges.

Method used

Multi-wire submerged arc welding rods and welding wires are used, with the chemical composition optimized to C: 0.03~0.12%, Si: 0.05~0.09%, Mn: 2.0~2.25%, P: ≤0.012%, S: ≤0.005%, Ni: 0.55~1.0%, Mo: 0.05~0.18%, Ti: 0.13~0.24%, B: 0.0005~0.0045%, V: 0.01~0.02%, Ca: ≤0.015%, Al: ≤0.05%, Zr: ≤0.005%, Cu: ≤0.05%, Cr: ≤0.05%. By controlling the proportion of alloying elements and using an Fe powder-MgO-SiO2-CaF2-Al2O3 alkaline sintering flux, high-efficiency welding can be achieved.

Benefits of technology

With a heat input of 50~150kJ/cm, the weld metal has a yield strength of 430~490MPa, a tensile strength of 525~570MPa, an elongation of 22~24%, and a KV2 impact toughness of 110~168J at -40℃. It has high welding efficiency, fine weld microstructure, and excellent crack resistance, making it suitable for the manufacture of large steel structures for bridges, ships, and buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116252067B_ABST
    Figure CN116252067B_ABST
Patent Text Reader

Abstract

The invention discloses a 500MPa multi-wire submerged arc welding wire rod capable of being welded at a heat input of 50-150kJ / cm. The wire rod is characterized in that the chemical composition of the wire rod comprises, by mass percentage, the following: C: 0.03-0.12, Si: 0.05-0.09, Mn: 2.0-2.25, P: ≤0.012, S: ≤0.005, Ni: 0.55-1.0, Mo: 0.05-0.18, Ti: 0.13-0.24, B: 0.0005-0.0045, V: 0.01-0.02, Ca: ≤0.015, Al: ≤0.05, Zr: ≤0.005, Re≤0.005, Cu≤0.05, Cr≤0.05, and the rest is Fe and unavoidable impurities. The present invention also discloses a 500MPa multi-wire submerged arc welding wire capable of being welded at a heat input of 50-150kJ / cm, which is made by drawing the above-mentioned wire rod. The welding wire of the present invention has excellent welding process performance at a heat input of 50-150kJ / cm, good molten pool fluidity, beautiful deposited metal molding, and excellent crack resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of welding materials and can be used for multi-wire eutectic pool high heat input welding by welding methods such as submerged arc welding and flux copper liner method. In particular, it relates to a multi-wire submerged arc automatic welding disc and welding wire which can be used for bridge steel Q345~Q420qEHW under the condition of 50~150kJ / cm heat input. Background Art

[0002] In the field of mechanical manufacturing such as bridges, shipbuilding, and construction, with the development of welding technology, while pursuing high-performance welded structures, we are also pursuing high efficiency in construction. Efficient welding helps shorten construction periods and save labor and component manufacturing costs.

[0003] Chinese invention patent application CN97104393.0 discloses a low-alloy high-strength and high-toughness submerged arc welding wire, whose composition is C: 0.06~0.12%; Mn: 1.20~1.80%; Si: 0.02~0.06%; Ni: 0.20~0.50%; Ti: 0.10~0.16; B: 0.006~0.01%, and the balance is iron and impurities. The welding wire reduces the content of C and Mn, controls the content of Si, reduces S and P, and adds 0.2~0.5% Ni, 0.10~0.16% Ti and 0.006~0.01% B, i.e., Mn-Ni-Ti-B system. It ensures the appropriate weld strength, increases the amount of acicular ferrite, and improves the low-temperature toughness of the weld metal. However, compared with the present invention, the welding wire does not add the Mo element, which can refine the structure and is beneficial to improving the low-temperature toughness. The welding wire of the invention is also said to be suitable for high heat input welding, but the mechanical properties of the welded joint at a welding heat input of 44 kJ / cm are only given in the examples. Similarly, in high heat input welding (50-150 kJ / cm) applicable to the present invention, 0.06-0.12% C and 1.2-1.8% Mn elements are seriously burned, which easily leads to insufficient weld metal strength. Therefore, in high heat input welding, it is necessary to add an appropriate amount of Mo element with relatively stable transition or increase the content of Mn element to compensate for the decrease in weld metal strength after the beneficial alloy elements are burned.

[0004] Chinese invention patent application CN201410666124.3 discloses a submerged arc welding wire with excellent low-temperature toughness for offshore platform construction, characterized in that the chemical composition of the welding wire contains C 0.01~0.15% by weight (%); Si 0.1~0.9%; Mn 0.5~2.0%; Ni0.1~1.5%; Mo 0.1~0.6%; Ti 0.01~0.25%; Al ≤0.01%, and CE is controlled to be ≤0.4%. However, in the submerged arc welding process, the Si element is generally transferred by the flux, and too high a content will reduce the low-temperature toughness of the weld. The upper limit of the Si element in the welding wire of the invention is relatively high; similarly, in the high heat input welding process, the cooling speed of the weld metal is slow, and the generation of proeutectoid ferrite at the grain boundary will have a great impact on the toughness of the weld metal. Therefore, adding an appropriate amount of B element in high heat input welding is beneficial to inhibit the formation of proeutectoid ferrite and side plate ferrite.

[0005] Chinese invention patent application CN200910046732.3 discloses a "high-toughness submerged arc welding wire" with moderate strength, high impact toughness and high wire energy resistance. By optimizing the carbon content, controlling the maximum upper limit of the silicon content, and combining the Mn-Ni system, it can effectively improve the low-temperature toughness and have appropriate yield strength and tensile strength. However, in the process of high heat input welding, when the welding heat input increases, the grain growth trend is more obvious. It is not possible to simply add Ni elements to refine the grains of the ferrite phase to improve toughness, and adding too much Ni elements will increase the cost of wire smelting. Similarly, this invention patent is applicable to welding heat input of 30~40kJ / cm, which is still a certain distance from high heat input welding.

[0006] Therefore, in order to improve the welding manufacturing efficiency of large steel structures in steel structure manufacturing enterprises such as bridges while meeting the requirements of relevant standards and specifications for the mechanical properties of welded joints, it is necessary to develop supporting domestic submerged arc automatic welding wires suitable for Q345~Q420qE level 50~150kJ / cm welding heat input. This is an important way to further improve welding efficiency, reduce production costs, improve the mechanical properties of welded joints and replace imported products. Summary of the invention

[0007] The problem to be solved by the present invention is to provide a 500MPa multi-wire submerged arc welding wire and a welding wire that can be welded at a heat input of 50-150kJ / cm, and is matched with a basic sintered flux of Fe powder-MgO-SiO2-CaF2-Al2O3. The submerged arc welding wire has a reasonable chemical composition, high deposition efficiency, excellent low-temperature toughness, strong adaptability to the welding heat input range, and is suitable for efficient welding and manufacturing of large steel structures in the fields of bridges, ships and buildings.

[0008] To solve the above technical problems, the technical solution adopted by the present invention is: a 500MPa multi-wire submerged arc welding wire rod that can be welded at a heat input of 50-150kJ / cm, the chemical composition of the wire rod comprising by mass percentage: C: 0.03-0.12, Si: 0.05-0.09, Mn: 2.0-2.25, P: ≤0.012, S: ≤0.005, Ni: 0.55-1.0, Mo: 0.05-0.18, Ti: 0.13-0.24, B: 0.0005-0.0045, V: 0.01-0.02, Ca: ≤0.015, Al: ≤0.05, Zr: ≤0.005, Re≤0.005, Cu≤0.05, Cr≤0.05, the rest are Fe and unavoidable impurities; in the above chemical composition: Pb+Sn+As+Sb+Bi≤120ppm, the contents of C, Si, Mn, Ni, Mo, Ti, B, Cr, Cu meet the requirements of: 4.5≤Ф≤7.0, 525.0≤θ≤570.0,

[0009] Among them, Ф=(Ni+4B+6Ti+2Mo) / (8Si+5Cu+3Cr); θ=8.8×(36.69+169.40C+5.44Mn+10.60Cr+2.62Ni+7.13Mo+1.20Ti).

[0010] The present invention also provides a 500MPa multi-wire submerged arc welding wire that can be welded at a heat input of 50-150kJ / cm, which is made by drawing the above-mentioned wire rod.

[0011] In the above technical scheme, the functions and mechanisms of each component are as follows:

[0012] C: Carbon C can expand the austenite phase area, improve the strength and hardness of the material, and improve the hardenability of the steel, but it is easy to cause welding cracks during welding and reduce the toughness and plasticity of the material. Therefore, the carbon content should not be too high. In the process of high heat input submerged arc welding, the carbon element has a large burnout, so in order to ensure appropriate strength and minimize the impact of carbon on toughness and crack resistance, the carbon content is controlled at 0.03~0.12%.

[0013] Si: Silicon is an effective precipitated deoxidizing element in the welding process. When silicon and manganese work together, they will form an oxidation complex, which is conducive to the deoxidation product floating out of the molten pool, and the deoxidation effect is significant. When the silicon content of the weld metal is too high, the toughness of the weld metal is significantly reduced. For submerged arc welding, the silicon in the weld metal after welding will be transferred from the base material and the submerged arc welding flux. Therefore, the silicon content in the welding wire composition is limited to ≤0.09%.

[0014] Mn: Manganese can expand the austenite phase area and reduce the bainite transformation temperature. At the same time, Mn can also improve hardenability and refine the structure. Mn improves the strength of weld metal through solid solution strengthening. The manganese content in this welding wire is controlled between 2.0~2.25%.

[0015] Mo: Mo is a carbide-forming element, which has a significant effect on improving strength and refining grains. Molybdenum is less burned during welding. Considering the effect of molybdenum on the properties of weld metal, the Mo content in the welding wire is limited to 0.15~0.35%.

[0016] Ni: Nickel is an austenite stabilizing element and can exist in austenite and ferrite in the form of solid solution with Fe, improving strength and low-temperature impact toughness. At the same time, Ni can also refine grains and inhibit the precipitation of ferrite at grain boundaries. In order to ensure that the weld metal has a certain degree of plasticity and toughness under high heat input welding conditions, 0.65~1.0% of nickel is added to toughen the ferrite matrix, reduce its brittle transition temperature, and improve low-temperature toughness.

[0017] Ti: Titanium is added to the submerged arc welding wire to form dispersed oxides and nitrides. These fine dispersed inclusions can promote the nucleation of acicular ferrite, inhibit grain boundary ferrite, effectively refine the grains, and improve the low-temperature toughness of the weld. In high heat input welding, Ti burns more seriously, and the amount of Ti added should be increased. Therefore, the Ti content in the welding wire composition is controlled at 0.13~0.24%.

[0018] Al: Aluminum is a ferrite-forming element, and its affinity with oxygen is greater than that of Ti. It can be used as an early deoxidizing element, and it plays a certain protective role in the transition of Ti elements. The Al2O3 generated by oxidation can be used as AF nucleation particles, effectively refining the weld structure. Excessive Al will reduce the austenite area, promote the formation of a large amount of massive ferrite, and reduce the impact toughness. Therefore, in terms of weld impact toughness, the Al content should be as low as possible, so the Al content in the welding wire composition is ≤0.05%.

[0019] Ca: Adding an appropriate amount of Ca can spheroidize the original strip-shaped MnS inclusions. At the same time, the CaS or CaO formed by Ca can be combined with other inclusions to induce the nucleation of AF, which is beneficial to improve the toughness of the deposited metal. However, when the Ca content exceeds 0.0015%, coarse inclusions will form in the weld and reduce the toughness of the weld metal. Therefore, the Ca content in this welding wire is controlled at ≤0.0015%.

[0020] B: Boron is a strong grain boundary segregation element, which can reduce the interface energy and the formation temperature of proeutectoid ferrite. Considering that B will be burned to a certain extent during high heat input welding, the B content in this welding wire is controlled at 0.0005~0.0045%.

[0021] S and P: They are harmful to the toughness of weld metal. Too high a content can easily cause cracks in the weld. Their content should be reduced as much as possible. The content of S element should not exceed 0.005%, and the content of P element should not exceed 0.012%.

[0022] Pb+Sn+As+Sb+Bi≤120ppm means that the sum of the five harmful elements of steel does not exceed 120ppm, indicating that the welding wire steel has good smelting quality and can avoid defects caused by harmful elements during welding. When the sum of the five harmful elements exceeds 120ppm, the welding quality of the weld may be reduced due to harmful elements, and even serious welding defects may occur. Pb is a heavy metal element with a soft texture and is difficult to form a solid solution with steel, so it is easy to form segregation, which is not conducive to the mechanical properties of the weld; the Sn element is easy to enrich at the grain boundary. Due to its low melting point, it will cause weld cracking under the action of welding stress; the As element is easy to segregate in steel, which increases the brittleness of the steel and reduces the mechanical properties of the weld; the Sb element will reduce the strength of the weld and increase the brittleness of the weld; the Bi element is difficult to form a solid solution with Fe and is easy to segregate at the grain boundary, which is not conducive to welding, and Bi will cause the brittleness of the weld and reduce the toughness of the weld.

[0023] In actual production, the strengthening methods of metal materials include solid solution strengthening, dislocation strengthening, precipitation and dispersion strengthening, and grain boundary strengthening. In weld metal, the main elements that cause solid solution strengthening are Mn, Si, Ni and Mo, while the oxides, carbides and nitrides formed by trace elements such as Ti and B in the weld can also pin dislocations and play a certain role in precipitation strengthening. However, the increase in strength due to solid solution strengthening is particularly significant, due to the atomic size effect, elastic modulus effect and solid solution ordering, which leads to body strengthening. When alloying elements alloy ferrite, their contribution to strength can be expressed by the following formula: , where K i is the strengthening coefficient of element i (MPa / wt%); C i is the weight percentage concentration of element i dissolved in ferrite. Assuming that the superposition of alloying elements is linear, the following formula can be listed to calculate the strength value caused by chemical composition:

[0024] . At the same time, during the high heat input welding process, the content of each alloy element transitioning to the weld metal also changes greatly, which is related to the oxidation and burning of the alloy elements during the welding heat process. According to welding metallurgy theory, at 1600°C, the order of the affinity of each element to oxygen from small to large is: Cu, Ni, Co, Fe, W, Mo, Cr, Mn, V, Si, Ti, Zr, Al. Since the concentration of Fe in the welding zone is the highest, some Fe must be oxidized; Ni is an element located to the right of Fe, and its affinity with oxygen is relatively small, so the oxidation loss is very small. Although Mo is located to the left of Fe, its affinity with oxygen is close to that of Fe, and its concentration in the molten droplet and the molten pool metal is relatively low, so the oxidation and burning are less, and the transition coefficient is relatively large; although the concentrations of Mn, Si, and Ti are not high, but due to their great affinity with oxygen, the oxidation and burning are more serious. In addition, Ti is very active and will react with nitrogen in the arc atmosphere to form TiN, etc., which will further reduce its alloy transition coefficient. Therefore, in high heat input welding, it is necessary to consider the effect of alloy elements on the strengthening and toughening of weld metal, as well as the element burnout caused by high heat input welding. Therefore, the transition margin of each alloy element after burnout by high heat input welding is combined with the strength increment caused by chemical composition to obtain a new expression for the strengthening and toughening factor θ:

[0025] . Among them, the strength factor θ satisfies 525.0≤θ≤570.0. By regulating the ratio of weld alloy elements according to the strengthening factor formula, the weld strength can meet the mechanical property requirements specified in the standard, and at the same time, the weld strength has an appropriate margin, avoiding low-strength matching and becoming a weak link in fracture; when the combined addition of alloy elements makes the θ value lower than the specified value, the weld strength will be too low to meet the mechanical property requirements, or the strength margin will be too small; when the addition of alloy elements makes the θ value higher than the specified value, the weld strength is too high, causing the problem of strength-toughness mismatch to be prominent, resulting in a significant decrease in the low-temperature impact toughness of the weld, and an imbalance in the strength-toughness matching of the weld. At the same time, it is bound to cause increased costs and waste of resources in terms of economy.

[0026] In addition, under high heat input welding conditions, the addition of alloy elements will affect the morphology and size of the weld structure. The welding wire optimizes the addition amount of Ni, Mo, Cr, Si, B, Ti, Cu, and Cr alloy elements to achieve the purpose of refining the weld structure of high heat input welding and improving its low-temperature impact toughness. The addition of alloy elements in the welding wire conforms to the ratio of 4.5≤Ф≤7.0, Ф=(Ni+4B+6Ti+2Mo) / (8Si+5Cu+3Cr). When the refinement factor Ф value is lower than the specified value, the degree of refinement of the weld structure by the alloy elements is insufficient, and there are still many coarse PF and other structures in the weld structure, and the proportion of AF structure still has room for improvement; when the refinement factor Ф value is higher than the specified value, the excessive content of alloy elements is also not conducive to the refinement of the weld structure. Excessive addition of the above alloys causes the phase transition temperature to drop significantly, the supercooling degree to increase, and a large amount of bainite structure begins to appear in the weld. The grain boundaries of the bainite structure do not have an obvious effect of hindering crack propagation. At the same time, the appearance of bainite structure increases the hardness of the structure and the internal stress of the weld metal, which is prone to serious deformation problems after high heat input welding.

[0027] Ni is an austenite stabilizing element and can be dissolved in ferrite and austenite. It can inhibit the formation of proeutectoid ferrite by lowering the phase transition temperature, promote the formation of acicular ferrite, and is beneficial to the refinement of the structure. Ti can form complex oxide inclusions, promote intracrystalline nucleation, and inhibit the formation of grain boundary ferrite. At the same time, Ti has a small atomic mass and can form TiC with C, which can fix a certain amount of C atoms. At the same time, the migration rate of TiC is fast, which can effectively avoid the formation of MA components. B can inhibit the coarse proeutectoid ferrite structure precipitated at the grain boundary and reduce the segregation of S and P elements at the grain boundary. In addition, within the control range of B content in this welding wire, the size of MA components can be inhibited. Although Mo can improve the strength of the weld, it is beneficial to the formation of MA components. Si will increase the phase transition point, coarsen the weld structure, and hinder the formation of carbides, which is beneficial to the formation of MA components. Cr will enrich C in austenite, which is beneficial to the formation of MA components. Cu will increase the austenite grain size, which is easy to cause the weld structure to coarsen.

[0028] The multi-wire submerged arc automatic welding wire of the present invention, in combination with the matching Fe powder-MgO-SiO2-CaF2-Al2O3 basic sintered flux, can be used for high heat input welding of Q345~Q420qEHW grade steel plates under 50~150kJ / cm welding heat input. The Mn-Mo-Ni-Ti-B alloy system is adopted, and under a wide range of heat input welding conditions, an appropriate amount of Ca element is adopted to modify the sulfide, and the weld strength under high heat input welding conditions is improved through the solid solution strengthening effect of Mn and Mo; the promotion effect of Ti on inclusions is fully utilized to increase the content of AF in the weld, and B can also reduce the amount of proeutectoid ferrite and reduce the damage of coarse structure to toughness; and the high Ni design can reduce the brittle transition temperature of the ferrite matrix by toughening it, and improve the stability of the low temperature impact toughness of the weld metal.

[0029] The manufacturing technology of the welding wire of the present invention is the same as the prior art. The alloy composition of the welding wire of the present invention is smelted and cast into steel ingots, then forged, rolled into wire rods, drawn into welding wires of corresponding sizes, and then copper plated and polished, wherein the copper plated layer has a thickness of 0.19-0.23 um, and finally rolled and packaged into finished products.

[0030] The beneficial effects of the present invention are:

[0031] (1) The welding wire of the present invention has a reasonable design of chemical composition, and the deposited metal obtained under a welding heat input of 50-150 kJ / cm has good process and mechanical properties. The deposited metal of the welding wire of the present invention has the following mechanical properties: yield strength R p0.2 / MPa: 430~490MPa, tensile strength R m / MPa: 525~570MPa, elongation A / %: 22~24%, -40℃KV2: 110~168J.

[0032] (2) The high-efficiency welding wire of the present invention can be applied to high heat input multi-wire eutectic pool welding methods such as submerged arc welding and flux copper backing method. The welding parameter adjustment range is wide. The welding process performance is excellent under the heat input of 50-150 kJ / cm, the molten pool fluidity is good, the deposited metal has beautiful shape, and the crack resistance is excellent.

[0033] (3) The welding wire alloy system of the present invention is reasonably regulated, and the wire rod smelting, rolling and welding wire drawing processes are easy to implement, with stable quality, and are suitable for large-scale promotion and application.

[0034] The present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is the weld structure diagram of Example 6 of the present invention;

[0036] Figure 2 This is a weld structure diagram of Example 7 of the present invention;

[0037] Figure 3 This is a weld structure diagram of Example 8 of the present invention;

[0038] Figure 4 This is a weld structure diagram of Example 9 of the present invention;

[0039] Figure 5 This is the weld structure diagram of comparative example 4 of the present invention;

[0040] Figure 6 This is the weld structure diagram of Comparative Example 5 of the present invention;

[0041] Figure 7 This is the weld structure diagram of comparative example 6 of the present invention. DETAILED DESCRIPTION

[0042] The invention provides a 500MPa multi-wire submerged arc welding wire rod which can be welded at a heat input of 50-150kJ / cm. The chemical composition of the wire rod comprises, by mass percentage, the following: C: 0.03-0.12, Si: 0.05-0.09, Mn: 2.0-2.25, P: ≤0.012, S: ≤0.005, Ni: 0.55-1.0, Mo: 0.05-0.18, Ti: 0.13-0.24, B: 0.0005-0.0045, V: 0.01-0.02, Ca: ≤0.015, Al: ≤0.05, Zr: ≤0.005, Re≤0.005, Cu≤0.05, Cr≤0.05, and the rest is Fe and unavoidable impurities.

[0043] In the above chemical composition: Pb+Sn+As+Sb+Bi≤120ppm.

[0044] The contents of C, Si, Mn, Ni, Mo, Ti, B, Cr and Cu meet the requirements of: 4.5≤Ф≤7.0, 525.0≤θ≤570.0.

[0045] Among them, Ф=(Ni+4B+6Ti+2Mo) / (8Si+5Cu+3Cr);

[0046] θ=8.8×(36.69+169.40C+5.44Mn+10.60Cr+2.62Ni+7.13Mo+1.20Ti).

[0047] The present invention also provides a 500MPa multi-wire submerged arc welding wire that can be welded at a heat input of 50-150kJ / cm, which is made by drawing the above-mentioned wire rod. The welding heat input of 50-100kJ / cm is suitable for double-wire submerged arc automatic welding, and the welding heat input of 100-150kJ / cm is suitable for three-wire submerged arc automatic welding. The basicity of the welding wire is 2.2≤B ⅡW For sintered flux with a temperature of ≤2.5, the proportion of acicular ferrite in the deposited metal of the welding wire shall not be less than 80%.

[0048] The present invention is described in detail below with reference to specific embodiments.

[0049] Embodiment: The chemical composition ratio of welding wire is shown in Table 1 and Table 3. According to the accurately calculated welding wire composition ratio, raw materials with low P and S impurity content are selected, the amount of alloy added is calculated, and a 75kg vacuum induction furnace is used to smelt welding wire steel. After charging, melting, and refining, it is cast into a steel ingot after the composition is qualified. After the steel ingot is forged into a square billet, it is rolled into an 8.5mm wire rod. The wire rod is subjected to one rough wire drawing and two fine wire drawing to form a 5.0mm submerged arc welding solid wire. The quality of the welding wire is stable. The surface of the welding wire is further copper-plated by a chemical copper plating method, and the copper plating thickness is controlled at 0.19~0.23um. The chemical composition ratio (mass percentage) of the specific embodiment of the welding wire of the present invention and the comparative example welding wire are shown in Table 1.

[0050] The above 10 welding wires (Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7, Example 8, Example 9, Example 10, Comparative Example 1, Comparative Example 2, Comparative Example 3, Comparative Example 4, Comparative Example 5, Comparative Example 6) were used to carry out double-wire cladding welding test according to the groove form shown in Table 2, with a heat input of 75 kJ / cm; three-wire cladding welding test was carried out according to the groove form shown in Table 4, with a welding heat input of 150 kJ / cm, and a specially formulated Fe powder-MgO-SiO2-CaF2-Al2O3 alkaline sintering flux was used for welding, and the layer temperature was controlled to be no more than 160°C.

[0051] Table 1 Chemical composition ratio (mass percentage) of submerged arc welding wires of Examples 1 to 5 of the present invention and Comparative Examples 1 to 3 (balance is Fe)

[0052] .

[0053] Table 2 Groove form of deposited metal test

[0054] .

[0055] Table 3 Chemical composition ratio (mass percentage) of submerged arc welding wires of Examples 6 to 10 of the present invention and Comparative Examples 1 to 3 (balance is Fe)

[0056] .

[0057] Table 4 Groove form of deposited metal test

[0058] .

[0059] Take samples from the deposited metal after welding to ensure that the parallel length is entirely composed of deposited metal. The sample size and test method are carried out in accordance with GB / T 228. The impact sample is cut from the center of the deposited metal. The longitudinal axis of the impact sample is perpendicular to the length direction of the deposited metal, the notch surface is perpendicular to the surface of the deposited metal, and the notch axis is located at the center of the deposited metal. The sample size is 10×10×55mm, and the impact test method is carried out in accordance with GB / T 229. The results of the tensile test and impact test of the deposited metal are shown in Table 5, and the average values ​​are in brackets in the table.

[0060] Table 5 Mechanical properties of deposited metal of welding wires of examples and comparative examples

[0061] .

[0062] See attached Figure 1-4 , the structure of the welding wire deposited weld of the embodiment of the present invention Figure 1 (Example 6), Figure 2 (Example 7), Figure 3 (Example 8), Figure 4 (Example 9), the microstructure is mainly composed of fine acicular ferrite and granular bainite, and the microstructure is evenly distributed; the acicular ferrite structure is a chain structure; it will make the crack propagation path tortuous, which can effectively hinder the crack propagation and improve the low-temperature impact toughness of the weld metal; the granular bainite structure can provide higher strength, and the contribution to toughness is weaker; therefore, even under the condition of high heat input of 150kJ / cm, excellent tensile strength and low-temperature impact toughness can still be obtained.

[0063] See attached Figure 5-7 , the deposited weld structure of the comparative example of the present invention Figure 5 (Comparative Example 4), Figure 6 (Comparative Example 5), Figure 7 (Comparative Example 6), the organizational composition is mainly proeutectoid ferrite, granular bainite and a small amount of acicular ferrite, and some of them contain a small amount of pearlite organization; its organization is relatively coarse and unevenly distributed; proeutectoid ferrite first precipitates at the original austenite grain boundary, the organization is relatively coarse, its strength is poor, and it cannot effectively hinder the crack propagation when the crack propagates. Pearlite is a layered product of ferrite and cementite stacking, has a high hardness, and is a hard and brittle organization; therefore, the low-temperature impact toughness of the comparative example is low.

[0064] It can be seen from the test results of the above examples that the mechanical properties of the deposited metal of the submerged arc welding solid wire of the present invention meet various regulatory requirements within the heat input range of 50-150 kJ / cm, that is, good strength and plasticity are obtained while also having excellent low-temperature impact toughness, and the KV2 of the weld metal at -40°C is 110-159 J. It can be applied to the production and efficient welding of large welded structural parts in industries such as bridges, ships and buildings.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A 500MPa multi-filament submerged arc welding wire rod capable of welding at a heat input of 50-150kJ / cm, characterized in that: The chemical composition of the wire rod includes by mass percentage: C: 0.03~0.12, Si: 0.05~0.09, Mn: 2.0~2.25, P: ≤0.012, S: ≤0.005, Ni: 0.55~1.0, Mo: 0.05~0.18, Ti: 0.13~0.24, B: 0.0005~0.0045, V: 0.01~0.02, Ca: ≤0.015, Al: ≤0.05, Zr: ≤0.005, Re≤0.005, Cu≤0.05, Cr≤0.05, and the rest is Fe and unavoidable impurities; Among the above chemical compositions: Pb+Sn+As+Sb+Bi≤120ppm, The contents of C, Si, Mn, Ni, Mo, Ti, B, Cr and Cu meet the requirements of: 4.5≤Ф≤7.0, 525.0≤θ≤570.0, Among them, Ф=(Ni+4B+6Ti+2Mo) / (8Si+5Cu+3Cr); θ=8.8×(36.69+169.40C+5.44Mn+10.60Cr+2.62Ni+7.13Mo+1.20Ti).

2. A 500MPa multi-wire submerged arc welding wire capable of welding at 50-150kJ / cm heat input, characterized in that: It is produced by drawing the wire rod as claimed in claim 1.

3. The 500MPa multi-wire submerged arc welding wire capable of being welded at a heat input of 50-150kJ / cm according to claim 2, characterized in that: The welding wire is matched with basicity B ⅡW The sintered flux has a viscosity of 2.2 to 2.5, and the proportion of acicular ferrite in the deposited metal of the welding wire is not less than 80%.

4. The 500MPa multi-wire submerged arc welding wire capable of being welded at a heat input of 50-150kJ / cm according to claim 3, characterized in that: The KV2 of the deposited metal of the welding wire is not less than 110J at -40°C.

5. The 500MPa multi-wire submerged arc welding wire capable of welding at a heat input of 50-150kJ / cm according to claim 3, characterized in that: The yield strength of the deposited metal of the welding wire is 430-490 MPa, the tensile strength is 525-570 MPa, and the elongation is 22-24%.

6. The 500MPa multi-wire submerged arc welding wire capable of being welded at a heat input of 50-150kJ / cm according to any one of claims 2-5, characterized in that: A copper plating layer is provided on the surface of the welding wire, and the thickness of the copper plating layer is 0.19-0.23 um.