A method for preparing Fe-based hydrogen-generating oxygen carrier
By using a combination method of phthalidite powder and ferric nitrate and aluminum nitrate in the preparation of Fe-based oxygen carrier, an iron-aluminum precipitation slurry was formed and calcined, which solved the problem of easy breakage and intimate bonding of the oxygen carrier. It significantly improves mechanical strength and improves the economic and stability of hydrogen production technology.
Patent Information
- Application Number
- CN202310034651.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-01-10
AI Technical Summary
The existing Fe-based hydrogen-producing oxygen carriers are prone to shatter during use and the Fe2O3 active components do not bind closely to alumina particles, resulting in insufficient mechanical strength in the hydrogen production process and affecting the economics of hydrogen production technology.
A new preparation method is adopted to uniformly disperse the phthalite powder in an inorganic saline aqueous solution, add ferrous nitrate and aluminum nitrate, and control the pH range between 7 and 11 to form a ferroaluminum precipitation slurry, and at high temperature The calcination treatment combines the glue solvent and extruder to significantly improve the mechanical strength of the oxygen carrier.
The prepared Fe-based oxygen carrier has high mechanical strength, which solves the problem of easy breakage of the oxygen carrier and intimate bonding of active components, and improves the economics of hydrogen production technology and the stability of the hydrogen production process.
Smart Images

Figure BDA0004048212090000111 
Figure BDA0004048212090000113
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an Fe-based hydrogen-producing oxygen carrier. Background Art
[0002] At present, nearly 80% of the world's energy consumption relies on traditional fossil fuels (coal, oil and natural gas, etc.). The burning of fossil fuels causes a large amount of CO2 emissions, exacerbating the greenhouse effect, so people try to seek green and environmentally friendly new energy to replace traditional fossil energy. Hydrogen energy is considered to be one of the most promising environmentally friendly energy sources in the future because of its high energy density and green and pollution-free combustion products. Therefore, how to produce hydrogen efficiently and sustainably is a key issue in realizing the widespread application of hydrogen energy. Compared with traditional hydrogen production processes, chemical looping hydrogen (CLH) is a new process that uses oxygen carriers as a source of pure oxygen. Due to its superior characteristics of system simplification and carbon capture, it has attracted great attention from scientific researchers and has been widely studied.
[0003] Chemical chain hydrogen production is a process based on redox reaction, in which hydrogen is produced by selecting appropriate oxygen carriers and cycling between different reactors. The following is an example of the process using the reaction equation of oxygen carriers as an example:
[0004] Fuel reactor 4Fe2O3+CH4→8FeO+2H2O+CO2
[0005] Steam Reactor:
[0006] Air Reactor:
[0007] The oxygen carrier not only provides lattice oxygen for the entire hydrogen production process to achieve oxygen transfer, but also participates in the reaction to provide heat and achieve heat transfer. In this process, the transfer of oxygen, participation in chemical reactions, and collisions with the vessel wall will cause the oxygen carrier itself to wear and break. Therefore, in order to allow the entire hydrogen production process to proceed normally and continuously, the oxygen carrier should have high mechanical strength (for example: the radial particle strength of the oxygen carrier is not less than 50N / cm), good oxygen transport capacity and other properties.
[0008] Fe-based oxygen carriers are low-priced, green, abundant in reserves, and have strong oxygen-releasing capacity. They are good materials suitable for use in the field of oxygen carriers, and Fe2O3 / Fe3O4 and Fe3O4 / FeO have different oxidation capacities. Therefore, Fe-based oxygen carriers have been widely used in chemical chain hydrogen production systems. Common oxygen carriers are mainly prepared by mechanical mixing. Although the oxygen carriers prepared by this method have high strength, since the precursor is obtained by physical mixing, there are problems such as loose bonding between active components and other oxide particles. For this reason, it is urgent to optimize the preparation to solve problems such as loose bonding between particles while meeting the mechanical strength requirements.
[0009] Based on the characteristics and existing problems of the above-mentioned Fe-based hydrogen production oxygen carrier, the present invention reports a new preparation method to synthesize Fe-based oxygen carriers with high mechanical strength properties to solve the problems of the oxygen carrier being easy to break during use and the Fe2O3 active component being loosely combined with the alumina particles. The solution to the above-mentioned problems is of great significance to improving the economic efficiency of hydrogen production technology. Summary of the invention
[0010] In view of the problems and shortcomings of the existing Fe-based oxygen carrier preparation method, the purpose of the present invention is to provide a new Fe-based hydrogen production oxygen carrier preparation method. The Fe-based oxygen carrier obtained by the present invention has the characteristics of tight combination of Fe2O3 active components and alumina particles, high mechanical strength, and simple preparation method.
[0011] The technical solutions adopted to solve the above problems are described below.
[0012] In a first aspect, the present invention provides a method for preparing an Fe-based oxygen carrier, the method comprising the following steps:
[0013] (a) adding pseudo-boehmite powder to an inorganic salt aqueous solution, stirring for 0.5 to 5 hours to uniformly disperse the powder to obtain an acidic colloid; the inorganic salt is iron nitrate nonahydrate and aluminum nitrate nonahydrate; based on the total mass of iron nitrate nonahydrate, aluminum nitrate nonahydrate and pseudo-boehmite being 100%, the mass of iron nitrate nonahydrate accounts for 20 to 25%, the mass of aluminum nitrate nonahydrate accounts for 63 to 70%, and the mass of pseudo-boehmite powder accounts for 8 to 13%;
[0014] (b) dissolving a precipitant in deionized water and stirring until dissolved to obtain an alkaline solution; the precipitant is one of NH4HCO3, (NH4)2CO3 and anhydrous Na2CO3, and the concentration of the alkaline solution is 1 mol / L to 5 mol / L;
[0015] (c) adding alkaline solution dropwise into the acidic colloid at a temperature of 30 to 95° C., controlling the pH value in the range of 7 to 11, to obtain an iron-aluminum precipitation slurry;
[0016] (d) aging the iron-aluminum precipitate slurry in an environment of 30 to 95° C. for 10 to 30 minutes;
[0017] (e) washing and filtering the aged iron-aluminum precipitate slurry to obtain a wet precursor, drying the wet precursor at 30 to 120° C. for 5 to 12 hours, and then grinding the wet precursor powder;
[0018] (f) dissolving a peptizing agent and an extrusion aid in deionized water to obtain a kneading liquid; the peptizing agent is a combination of citric acid and nitric acid; the extrusion aid is a combination of one or more of polyethylene glycol 400, sesbania powder, methyl cellulose and polycarboxylic acid; in the kneading liquid, the mass percentages of the peptizing agent and the extrusion aid are 1wt% to 5wt% and 1wt% to 10wt%, respectively;
[0019] (g) mixing the precursor powder obtained in step (e) with a binder, adding a kneading liquid dropwise to the mixture of the precursor powder and the binder in a certain proportion, and continuously extruding and kneading to fully mix the powder particles with the kneading liquid to obtain a wet powder mass; the binder is pseudo-boehmite or a mixture of pseudo-boehmite and montmorillonite, and the mass ratio of the precursor powder to the binder is 1:0.2-0.5 (preferably 1:0.3); the water-powder mass ratio of the kneading liquid to the mixture of the precursor powder and the binder is 0.5-2, preferably 1.1;
[0020] (h) extruding the wet powder mass into wet strips of uniform thickness, and treating the wet strips at 30 to 100° C. for 6 to 12 hours to obtain a green body;
[0021] (i) The green body is subjected to high temperature calcination treatment at 600-1100° C. for 4-6 h (preferably 5 h) to obtain the Fe-based oxygen carrier.
[0022] The oxygen carrier of the present invention mainly contains Al2O3 and Fe2O3, wherein Fe2O3 is an active component.
[0023] Furthermore, the inorganic salt aqueous solution described in step (a) is preferably prepared by the following method: Fe-containing inorganic salt and Al-containing inorganic salt are respectively prepared with deionized water to form an Fe-containing inorganic salt solution and an Al-containing inorganic salt solution with a concentration of 0.2 mol / L to 0.3 mol / L (more preferably 0.25 mol / L), and then the two solutions are mixed to obtain the inorganic salt aqueous solution.
[0024] Furthermore, the precipitant described in step (b) is preferably (NH4)2CO3.
[0025] Furthermore, the concentration of the alkali solution in step (b) is preferably 1 mol / L to 3 mol / L, more preferably 2 mol / L.
[0026] Furthermore, the aging time in step (d) is preferably 10 to 30 minutes, more preferably 10 minutes.
[0027] Furthermore, the particle size range of the precursor powder in step (e) is preferably 140-160 mesh.
[0028] Furthermore, the extrusion aid in step (f) is preferably polyethylene glycol 400.
[0029] Furthermore, in step (f), the peptizing agent preferably comprises nitric acid and citric acid in a mixing mass ratio of 1:1 to 2.
[0030] Furthermore, in step (f), the kneading liquid is prepared from nitric acid, citric acid, polyethylene glycol 400 and deionized water, wherein the ratio of nitric acid, citric acid, polyethylene glycol 400 and deionized water is 10.5:12.2:21:454 based on the mass ratio of 68wt% concentrated nitric acid, citric acid, polyethylene glycol 400 and deionized water.
[0031] Furthermore, the binder in step (g) is preferably a mixture of pseudo-boehmite and montmorillonite, and more preferably the mass ratio of the mixture of pseudo-boehmite and montmorillonite is 2:1.
[0032] Furthermore, in step (g), the water-powder mass ratio of the kneading liquid to the mixture of the precursor powder and the binder is 1.0-1.5, more preferably 1.1.
[0033] Furthermore, the high temperature calcination atmosphere in step (i) is preferably air, the calcination temperature is preferably 1000° C., and the calcination time is preferably 5 hours.
[0034] The radial particle strength of the Fe-based oxygen carrier prepared by the invention is not less than 50N / cm.
[0035] Compared with the prior art, the present invention has the following advantages:
[0036] (1) The Fe-based oxygen carrier reported in the present invention adds pseudo-boehmite during the preparation of the precursor, and adopts a method of first peptizing and then precipitation, so that the active components of the oxygen carrier and alumina are more closely combined, and the problem of difficulty in forming the precursor prepared by a simple co-precipitation method is solved;
[0037] (2) The Fe-based oxygen carrier prepared by the method reported in the present invention has high strength and less dust, which solves the problem of easy breakage faced by the hydrogen-producing oxygen carrier due to its own insufficient strength. DETAILED DESCRIPTION
[0038] The technical solution of the present invention is further described below with specific embodiments, but the protection scope of the present invention is not limited by the following embodiments.
[0039] Example 1
[0040] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C, adjust the pH value to 7.5-8.5, and obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0041] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid and polyethylene glycol 400 are 1%, 2% and 4% respectively; 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.1, and the powder particles are continuously squeezed and kneaded to fully mix the powder particles with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a wet strip with uniform thickness, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 600°C for 5 hours to obtain the Fe-based oxygen carrier Fe-1.1-600. After strength testing, its lateral compressive strength is 92.5 (N / cm).
[0042] Example 2
[0043] Weigh 30.36g of Fe(NO3)3·9H2O and 88.30g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare 0.25mol / L iron-containing solution and aluminum-containing solution respectively, then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12g of pseudo-boehmite powder and disperse it in the inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid. Weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkaline solution with a concentration of 2mol / L. At 85°C, an alkali solution is added dropwise to the acidic colloid to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitate slurry, and then aged at 85°C for 10 minutes; the iron-aluminum precipitate slurry is washed three times with deionized water, washed twice with anhydrous ethanol, and then filtered to obtain a wet precursor, which is dried at 100°C for 5 hours and then ground to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and the aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0044] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 were dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid, and polyethylene glycol 400 were 1%, 2%, and 4%, respectively. 5 g of precursor powder, 1 g of pseudo-boehmite, and 0.5 g of montmorillonite were weighed and mixed, and the mixed solution A was added dropwise according to a water-powder mass ratio of 1.4, and the mixture was continuously squeezed and kneaded to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass was squeezed into a uniform wet strip, and dried at 35°C for 12 hours to obtain a green body; the green body was calcined at 600°C for 5 hours to obtain an Fe-based oxygen carrier (Fe-1.4-600). After strength testing, its lateral compressive strength was 65.7 N / cm.
[0045] Example 3
[0046] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0047] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid and polyethylene glycol 400 are 1%, 2% and 4% respectively; 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.94, and the mixture is continuously squeezed and kneaded to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a wet strip with uniform thickness, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 600°C for 5 hours to obtain an Fe-based oxygen carrier Fe-1.94-600. After strength testing, its lateral compressive strength is 48.1 (N / cm).
[0048] Example 4
[0049] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0050] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid and polyethylene glycol 400 are 1%, 2% and 4% respectively; 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.4, and the mixture is continuously squeezed and kneaded to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a wet strip with uniform thickness, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 1000°C for 5 hours to obtain an Fe-based oxygen carrier Fe-1.4-1000. After strength testing, its lateral compressive strength is 150.2 (N / cm).
[0051] Example 5
[0052] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0053] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid and polyethylene glycol 400 are 1%, 2% and 4% respectively; 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.1, and the powder particles are continuously squeezed and kneaded to fully mix the powder particles with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a wet strip with uniform thickness, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 1000°C for 5 hours to obtain an Fe-based oxygen carrier Fe-1.1-1000. After strength testing, its lateral compressive strength is 154.2 (N / cm).
[0054] Comparative Example 1
[0055] Weigh 30.36g Fe(NO3)3·9H2O and 176.6g Al(NO3)3·9H2O and dissolve them in deionized water to prepare 0.25mol / L iron-containing solution and aluminum-containing solution respectively, then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh (NH4)2CO3 and dissolve it in deionized water, stir and prepare an alkali solution with a concentration of 2mol / L; add the alkali solution dropwise to the inorganic salt aqueous solution at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitate slurry; then age at 85°C for 10min; wash the iron-aluminum slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0056] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid and polyethylene glycol 400 are 1%, 2% and 4% respectively; 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.1, and the mixture is continuously squeezed and kneaded to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a uniform wet strip, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 600°C for 5 hours to obtain an Fe-based oxygen carrier. The sample prepared by this method is very fragile, and after strength testing, its lateral compressive strength is less than 10 (N / cm).
[0057] By comparing Example 1 with Comparative Example 1, it can be seen that adding pseudo-boehmite powder to the Fe / Al mixed solution to prepare an acidic colloid can significantly improve the lateral compressive strength of the Fe-based oxygen carrier finally prepared.
[0058] Comparative Example 2
[0059] Weigh 30.36g Fe(NO3)3·9H2O and 176.6g Al(NO3)3·9H2O and dissolve them in deionized water to prepare 0.25mol / L iron-containing solution and aluminum-containing solution respectively, then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh (NH4)2CO3 and dissolve it in deionized water, stir and prepare 2mol / L alkali solution; add the alkali solution dropwise to the Fe / Al mixed solution at 85℃ to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitate slurry; then age at 85℃ for 10min; wash the iron-aluminum precipitate slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter to obtain a wet precursor, dry it at 100℃ for 5 hours, and grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated as iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0060] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid and polyethylene glycol 400 are 1%, 2% and 4%, respectively; 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.4, and the mixture is continuously squeezed and kneaded to fully mix the powder particles with the kneading liquid to obtain a wet powder mass; the wet powder mass is extruded into strips, and the sample prepared by this method cannot be formed.
[0061] In Comparative Example 2, no pseudo-boehmite is added to the Fe / Al mixed solution, and the precursor is obtained by only precipitating iron and aluminum. The sample prepared by this method cannot be formed. By comparing Example 2 and Comparative Example 2, it can be seen that adding an acidic colloid made of pseudo-boehmite during precipitation can make the sample better formed.
[0062] Comparative Example 3
[0063] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0064] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid, and polyethylene glycol 400 are 1%, 2%, and 4%, respectively. 5 g of precursor powder is weighed, and the mixed solution A is added dropwise according to a water-powder mass ratio of 1.1, and the powder particles are continuously squeezed and kneaded to fully mix the powder particles with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a uniform wet strip, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 600°C for 5 hours to obtain an Fe-based oxygen carrier (Fe-blank-1.1-600). The sample prepared by this method is very fragile, and after strength testing, its lateral compressive strength is less than 10 (N / cm).
[0065] By comparing Example 1 with Comparative Example 3, it can be seen that the addition of the binder can significantly improve the lateral compressive strength of the Fe-based oxygen carrier finally prepared.
[0066] Comparative Example 4
[0067] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry three times with deionized water, wash it twice with anhydrous ethanol, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh (the iron species and aluminum species in the precursor are calculated in the form of iron oxide and aluminum oxide, and the mass ratio is 2:8);
[0068] 10.5 g of 68% GR purity concentrated nitric acid solution, 12.2 g of GR purity citric acid solid, and 21 g of AR purity polyethylene glycol 400 were dissolved in 454 g of deionized water to obtain a mixed solution A, wherein the mass percentages of nitric acid, citric acid, and polyethylene glycol 400 were 1%, 2%, and 4%, respectively. 5 g of precursor powder was weighed, and the mixed solution A was added dropwise according to a water-powder mass ratio of 1.4, and the mixture was squeezed and kneaded continuously to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass was extruded into strips, and the sample prepared by this method could not be formed.
[0069] By comparing Example 2 and Comparative Example 4, it can be seen that the addition of a binder has an important influence on whether the wet powder dough can be extruded.
[0070] Comparative Example 5
[0071] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry with deionized water three times, wash it with anhydrous ethanol twice, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh;
[0072] 10.5 g of 68% GR purity concentrated nitric acid solution and 21 g of AR purity polyethylene glycol 400 are dissolved in 454 g of deionized water to obtain a mixed solution B, wherein the mass percentages of nitric acid and polyethylene glycol 400 are 1% and 4% respectively. 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite are weighed and mixed, and the mixed solution B is added dropwise according to a water-powder mass ratio of 1.1, and the mixture is continuously squeezed and kneaded to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass is squeezed into a wet strip of uniform thickness, and dried at 35°C for 12 hours to obtain a green body; the green body is calcined at 600°C for 5 hours to obtain Fe-based oxygen carrier Fe-1.1-B-600. The sample prepared by this method is very fragile, and after strength testing, its lateral compressive strength is less than 10 (N / cm).
[0073] By comparing Example 1 and Comparative Example 5, it can be seen that adding citric acid as a peptizing agent can significantly improve the lateral compressive strength of the Fe-based oxygen carrier finally prepared. The mechanical strength of the sample prepared by using a kneading liquid containing only nitric acid and polyethylene glycol 400 is significantly poor.
[0074] Comparative Example 6
[0075] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitate slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitate slurry with deionized water three times, wash it with anhydrous ethanol twice, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh;
[0076] 12.2 g of GR purity citric acid solid and 21 g of AR purity polyethylene glycol 400 were dissolved in 454 g of deionized water to obtain a mixed solution C, wherein the mass percentages of citric acid and polyethylene glycol 400 were 3% and 4% respectively. 5 g of precursor powder, 1 g of pseudo-boehmite and 0.5 g of montmorillonite were weighed and mixed, and the mixed solution C was added dropwise according to a water-powder mass ratio of 1.1, and the mixture was continuously squeezed and kneaded to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; the wet powder mass was squeezed into a wet strip with uniform thickness, and dried at 35°C for 12 hours to obtain a green body; the green body was calcined at 600°C for 5 hours to obtain the Fe-based oxygen carrier Fe-1.1-C-600. The sample prepared by this method is very fragile, and after strength testing, its lateral compressive strength is less than 10 (N / cm).
[0077] By comparing Example 1 and Comparative Example 6, it can be seen that adding nitric acid as a peptizing agent can significantly improve the lateral compressive strength of the Fe-based oxygen carrier finally prepared. The mechanical strength of the sample prepared by using a kneading liquid containing only polyethylene glycol 400 and citric acid is significantly poor.
[0078] Comparative Example 7
[0079] Weigh 30.36 g of Fe(NO3)3·9H2O and 88.30 g of Al(NO3)3·9H2O and dissolve them in deionized water to prepare an iron-containing solution and an aluminum-containing solution with a concentration of 0.25 mol / L respectively, and then mix the aluminum-containing solution and the iron-containing solution to obtain an inorganic salt aqueous solution. Weigh 14.12 grams of pseudo-boehmite powder and disperse it in an inorganic salt aqueous solution, stir it for 4 hours to make it evenly dispersed to obtain an acidic colloid; weigh (NH4)2CO3 and dissolve it in deionized water, stir to prepare an alkali solution with a concentration of 2 mol / L; add the alkali solution dropwise to the acidic colloid at 85°C to adjust the pH value to 7.5-8.5 to obtain an iron-aluminum precipitation slurry; then, age it at 85°C for 10 minutes; wash the iron-aluminum precipitation slurry with deionized water three times, wash it with anhydrous ethanol twice, and then filter it to obtain a wet precursor, dry it at 100°C for 5 hours, and then grind it to obtain a precursor powder with a particle size of 140-160 mesh;
[0080] Take 10.5 grams of 68% GR purity concentrated nitric acid solution and 12.2 grams of GR purity citric acid solid and dissolve them in 454 grams of deionized water to obtain a mixed solution D, in which the mass percentages of nitric acid and citric acid are 1% and 3% respectively. Weigh 5 grams of precursor powder, 1 gram of pseudo-boehmite and 0.5 grams of montmorillonite, mix them, add mixed solution D dropwise according to the water-powder mass ratio of 1.1, and continuously squeeze and knead to make the powder particles fully mixed with the kneading liquid to obtain a wet powder mass; squeeze the wet powder mass into a uniform wet strip, and dry it at 35°C for 12 hours to obtain a green body; calcine the green body at 600°C for 5 hours to obtain Fe-based oxygen carrier Fe-1.1-D-600. The sample prepared by this method is very fragile. After strength testing, its lateral compressive strength is less than 10 (N / cm).
[0081] By comparing Example 1 and Comparative Example 7, it can be seen that adding polyethylene glycol 400 as an extrusion aid can significantly improve the lateral compressive strength of the Fe-based oxygen carrier finally prepared. The mechanical strength of the sample prepared by using a kneading liquid containing only nitric acid and citric acid is significantly poor.
[0082] The present invention uses a YHKC-2A particle strength tester (Taizhou Yinhe Instrument Factory) to measure the lateral compression strength of the Fe-based oxygen carriers prepared in Examples 1-5 and Comparative Examples 1-7.
[0083] First, the prepared Fe-based oxygen carrier is divided into 10-15 particles with a relatively uniform length of 4mm-6mm, and the length is measured by a vernier caliper and recorded as l (mm). Then, it is placed in the center of the tray of the particle strength tester, and then the peak value F′ (N) when the particles are crushed is measured and recorded. Finally, the lateral pressure resistance of the final oxygen carrier is calculated according to the determination standard of the crushing force of catalyst particles in the Chemical Industry Standard of the People's Republic of China (HGT2782-2011).
[0084] The specific calculation is as follows:
[0085] (1) Radial crushing resistance F, expressed in Newton per centimeter (N / cm)
[0086]
[0087] Where:
[0088] F'-The value displayed by the intelligent particle strength tester when the sample is broken, in Newton (N)
[0089] l-Numerical value of sample length, in centimeters (cm)
[0090] (2) Average radial crushing strength The value is expressed in Newton per centimeter (N / cm)
[0091]
[0092] Where:
[0093] F i -The radial crushing resistance of the ith particle, in Newton per centimeter (N / cm);
[0094] n-Number of particles measured in the sample.
[0095] The above experimental results show that the Fe-based oxygen carrier obtained by the preparation method shown in the present invention has high mechanical strength. At the same time, under the same calcination temperature, appropriately reducing the water-powder ratio is conducive to improving the strength of the oxygen carrier; after extrusion molding of the same precursor powder and the same water-powder ratio, the mechanical strength of the oxygen carrier increases significantly as the calcination temperature increases.
Claims
1. A method for preparing an Fe-based oxygen carrier, characterized in that: The preparation method comprises the following steps: (a) adding pseudo-boehmite powder to an inorganic salt aqueous solution, stirring for 0.5 to 5 hours to uniformly disperse the powder to obtain an acidic colloid; the inorganic salt is iron nitrate nonahydrate and aluminum nitrate nonahydrate; based on the total mass of iron nitrate nonahydrate, aluminum nitrate nonahydrate and pseudo-boehmite being 100%, the mass of iron nitrate nonahydrate accounts for 20 to 25%, the mass of aluminum nitrate nonahydrate accounts for 63 to 70%, and the mass of pseudo-boehmite powder accounts for 8 to 13%; (b) dissolving a precipitant in deionized water and stirring until dissolved to obtain an alkaline solution; the precipitant is one of NH4HCO3, (NH4)2CO3 and anhydrous Na2CO3, and the concentration of the alkaline solution is 1 mol / L to 5 mol / L; (c) adding alkaline solution dropwise to the acidic colloid at a temperature of 30 to 95° C., controlling the pH value in the range of 7 to 11, to obtain an iron-aluminum precipitation slurry; (d) aging the iron-aluminum precipitate slurry in an environment of 30 to 95° C. for 10 to 30 minutes; (e) washing and filtering the aged iron-aluminum precipitate slurry to obtain a wet precursor, drying the wet precursor at 30 to 120° C. for 5 to 12 hours, and then grinding the wet precursor powder; (f) dissolving a peptizing agent and an extrusion aid in deionized water to obtain a kneading liquid; the peptizing agent is a combination of citric acid and nitric acid; the extrusion aid is a combination of one or more of polyethylene glycol 400, sesbania powder, methyl cellulose and polycarboxylic acid; in the kneading liquid, the mass percentages of the peptizing agent and the extrusion aid are 1wt% to 5wt% and 1wt% to 10wt%, respectively; (g) mixing the precursor powder obtained in step (e) with a binder, adding a kneading liquid dropwise to the mixture of the precursor powder and the binder in a certain proportion, and continuously extruding and kneading to fully mix the powder particles with the kneading liquid to obtain a wet powder mass; the binder is pseudo-boehmite or a mixture of pseudo-boehmite and montmorillonite, the mass ratio of the precursor powder to the binder is 1:0.2-0.5; the mass ratio of the kneading liquid to the mixture of the precursor powder and the binder is 0.5-2; (h) extruding the wet powder mass into wet strips of uniform thickness, and treating the wet strips at 30 to 100° C. for 6 to 12 hours to obtain a green body; (i) The green body is placed in a high temperature calcination treatment at 600-1100° C. for 4-6 hours to obtain the Fe-based oxygen carrier.
2. The preparation method according to claim 1, characterized in that: The inorganic salt aqueous solution described in step (a) is prepared by the following method: Fe-containing inorganic salt and Al-containing inorganic salt are respectively prepared into Fe-containing inorganic salt solution and Al-containing inorganic salt solution with a concentration of 0.2 mol / L to 0.3 mol / L with deionized water, and then the two solutions are mixed to obtain the inorganic salt aqueous solution.
3. The preparation method according to claim 1, characterized in that: The concentration of the alkali solution in step (b) is 1 mol / L to 3 mol / L.
4. The preparation method according to claim 1, characterized in that: In step (f), the mixing mass ratio of nitric acid to citric acid in the peptizing agent is 1:1-2.
5. The preparation method according to claim 4, characterized in that: In step (f), the kneading liquid is prepared from nitric acid, citric acid, polyethylene glycol 400 and deionized water, wherein the ratio of nitric acid, citric acid, polyethylene glycol 400 and deionized water is 10.5:12.2:21:454 based on the mass ratio of 68wt% concentrated nitric acid, citric acid, polyethylene glycol 400 and deionized water.
6. The preparation method according to claim 1, characterized in that: The binder in step (g) is a mixture of pseudo-boehmite and montmorillonite, wherein the mass ratio of the pseudo-boehmite to montmorillonite is 2:
1.
7. The preparation method according to claim 1, characterized in that: The water-powder mass ratio of the kneading liquid to the mixture of the precursor powder and the binder in step (g) is 1.0-1.
5.
8. The preparation method according to claim 7, characterized in that: The water-powder mass ratio of the kneading liquid to the mixture of the precursor powder and the binder in step (g) is 1.
1.
9. The preparation method according to claim 1, characterized in that: In step (i), the high temperature calcination atmosphere is air, and the calcination treatment time is 5 hours.
10. The preparation method according to claim 9, characterized in that: In step (i), the calcination temperature is 1000° C. and the calcination time is 5 hours.