A biochar-based titanium dioxide composite photocatalyst and its preparation method and application

Through the preparation of biochar-based titanium dioxide composite photocatalyst, the modification of phosphoric acid and sodium dodecyl sulfate and combined with titanium dioxide catalysis, the problem that adsorbent materials cannot effectively degrade organic pollutants is solved, and efficient adsorption and photocatalytic degradation are achieved, reducing Dispose of costs and resource utilization of biological waste.

CN116272934BActive Publication Date: 2024-11-19SHANGHAI INST OF TECH
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310099123.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-09
Publication Date
2024-11-19
Estimated Expiration
2043-02-09

AI Technical Summary

Technical Problem

Existing adsorption materials can only adsorb and cannot effectively degrade organic pollutants. In addition, activated carbon is prone to adsorption and saturation, resulting in a decrease in adsorption performance, high treatment costs, and serious problems in resource waste and secondary pollution.

Method used

Using biochar-based titanium dioxide composite photocatalyst, the formation of rich layered structures and large pore sizes through phosphoric acid modification and sodium dodecyl sulfate supplementary modification, enhance adsorption capacity, and accelerate the light of organic pollutants through the catalytic active center of titanium dioxide. degradation.

Benefits of technology

It achieves efficient adsorption and photocatalytic degradation, excellent degradation performance of organic pollutants, high utilization efficiency, extends the service life of the catalyst, reduces the treatment cost, and resources the utilization of biological waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116272934B_ABST
    Figure CN116272934B_ABST
Patent Text Reader

Abstract

The present invention provides a biochar-based titanium dioxide composite photocatalyst and a preparation method and application thereof, belonging to the technical field of photocatalysts. The present invention mixes peanut shell particles, titanium dioxide and sodium dodecyl sulfate to obtain a mixture; the mixture is activated and roasted in sequence to obtain a biochar-based titanium dioxide composite photocatalyst. The biochar-based titanium dioxide composite photocatalyst obtained by the present invention has good adsorption and photocatalytic degradation of methylene blue, high reuse rate, and the degradation efficiency can still reach more than 90% after being recycled for 3 times. The present invention provides an effective way to recycle biomass waste such as peanut shells, and better solves the problem of low reuse rate of biochar.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photocatalysts, and in particular to a biochar-based titanium dioxide composite photocatalyst and a preparation method and application thereof. Background Art

[0002] Only a small part of peanut shells is used to make roughage or fuel, and most of the rest is thrown away, resulting in a huge waste of resources and causing certain impacts on environmental pollution. Many researchers have studied the development and utilization of peanut shells and found that they can be used in agriculture, food, medicine, chemical industry, light industry and other fields, and have achieved many research results. Peanut shells contain a large amount of polyphenols and cellulose substances, which have a great effect on the adsorption performance of peanut shells. For example, after treatment, they can be used to adsorb and remove organic pollutants in wastewater (Feng Lingling, Yu Zhimin, Wei Xinlai, et al. Research status of peanut shell activation and adsorption of heavy metals in wastewater [J]. Environmental Science and Technology, 2015, 21(05): 39-45).

[0003] Industrial wastewater is continuously discharged into the natural environment, causing irreversible damage to water resources and soil resources. Among them, the treatment of organic dyes and their emissions has attracted widespread attention. Methylene blue (MB) is one of the dyes commonly used in industrial printing and dyeing. It is a cationic organic dye with an aromatic structure. It is used as the main raw material for wood, cotton, silk, textiles, printing, pesticides, pulp and paper, cosmetics, food processing and research laboratories. Its aqueous solution is alkaline and toxic. It is a difficult-to-degrade organic compound (YUEN FK, HAMEED B H. Recent developments in the preparation and regeneration of activated carbons by microwaves[J. Advances in Colloid and Interface Science, 2009, 149(1-2):19-27).

[0004] To date, various wastewater treatment technologies have received widespread attention, such as chemical coagulation, adsorption, coagulation-flocculation, photocatalyst (Lu Lili, Shan Rui, He Mingyang, et al. Photocatalytic degradation of methyl orange by a novel TiO2 / biochar composite catalyst [J]. Acta Energiae Solaris Sinica, 2021, 42(04): 32-39), ozone, etc. However, they all have problems such as energy consumption, economy, and instability in large-scale application. Among the various physical, chemical, and biological technologies currently being explored, adsorption is widely considered to be the most effective and promising method. Adsorption is suitable for removing dyes from water and wastewater. Many materials with adsorption properties have been widely studied as dye adsorbents, such as carbon nanotubes, graphene oxide, high molecular weight polymers, porous zeolites, metal oxides, and biochar. Among them, biochar has been widely studied due to its large specific surface area and pore volume.

[0005] Biochar adsorption is the transfer of adsorbed substances from the liquid phase to the solid phase, which cannot fundamentally degrade organic matter. Moreover, activated carbon is easily saturated with adsorption, resulting in a sharp decline in adsorption performance. In addition, replacing new carbon will lead to excessively high treatment costs, and discarding saturated activated carbon will easily cause problems such as waste of resources and secondary pollution, which limit the promotion and application of pure activated carbon (Fu Xiaolin, Jia Biao, Wang Zhanxin, et al. Research progress on activated carbon regeneration methods and their applications in water treatment [J]. Industrial Water and Wastewater, 2020, 51(3): 1-5). Therefore, how to achieve the combination of photodegradation and physical adsorption to obtain a catalyst material with excellent degradation performance and high utilization efficiency is a technical problem that needs to be solved at present. Summary of the invention

[0006] The purpose of the present invention is to provide a biochar-based titanium dioxide composite photocatalyst and a preparation method and application thereof, so as to solve the technical problem that existing adsorption materials can only adsorb but not effectively degrade organic pollutants.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a biochar-based titanium dioxide composite photocatalyst, comprising the following steps:

[0009] 1) mixing peanut shell particles, titanium dioxide and sodium lauryl sulfate to obtain a mixture;

[0010] 2) The mixture is activated and calcined in sequence to obtain a biochar-based titanium dioxide composite photocatalyst.

[0011] Furthermore, the particle size of the peanut shell particles is 200-300 meshes, and the mass ratio of the peanut shell particles, titanium dioxide and sodium dodecyl sulfate is 1-3: 0.05-0.2: 0.1-0.3.

[0012] Furthermore, in step 2), a phosphoric acid solution is used as an activating agent in the activation treatment, and the concentration of the phosphoric acid solution is 80-90 wt %.

[0013] Furthermore, the temperature of the activation treatment is 20-30° C., and the time of the activation treatment is 0.5-2 h.

[0014] Furthermore, in step 2), the mass volume ratio of the mixture to the phosphoric acid solution is 1-3.5 g: 3-10 mL.

[0015] Furthermore, in the step 2), the calcination treatment is performed under a protective atmosphere, and the protective atmosphere contains nitrogen and / or argon.

[0016] Furthermore, the calcination temperature is 400-500°C, the calcination time is 0.5-2h, and the calcination heating rate is 8-12°C / min.

[0017] The invention provides a biochar-based titanium dioxide composite photocatalyst.

[0018] The invention provides an application of a biochar-based titanium dioxide composite photocatalyst in photocatalytic degradation of organic pollutants.

[0019] Beneficial effects of the present invention:

[0020] The present invention uses phosphoric acid as the main modifier, sodium dodecyl sulfate as the auxiliary modifier, and titanium dioxide as the catalytic active center to prepare a biochar composite photocatalytic material. First, phosphoric acid can increase the acidity of the biochar surface, etch the biochar precursor, and form a rich layered structure; secondly, phosphoric acid will undergo a cross-linking reaction with the biomass surface during the heating process to become a polycondensate, effectively preventing the biochar pores from collapsing and forming a large-pore material; finally, phosphoric acid can activate the biochar surface and increase the oxygen-containing functional groups on the biochar surface, thereby enhancing the adsorption capacity of the biochar. Specifically, the polyphosphoric acid and phosphate generated by phosphoric acid during the pyrolysis process can provide support in the pores, prevent the pores from collapsing and expand the specific surface area of ​​the biochar; phosphoric acid helps the decomposition of lignocellulose, aromatic substances, and aliphatic substances, and forms functional groups such as carbonyl, hydroxyl, and carboxyl on the biochar surface, thereby enhancing the hydrophilicity of the biochar. According to the swelling effect, sodium dodecyl sulfate polycondenses in the biomass, reduces pore collapse, and forms a larger pore size, which is conducive to the adsorption of methylene blue macromolecules. Titanium dioxide is attached to the surface of biochar by impregnation to form a large number of catalytic active centers, which photocatalytically degrade the adsorbed methylene blue.

[0021] The present invention also has the following beneficial effects:

[0022] Environmental aspects: The present invention provides a method for the resource utilization of biological waste, which reduces the cost of sewage treatment while utilizing biomass waste as a resource.

[0023] Technical aspects: The pore size of phosphoric acid-modified biochar is large, and there are a large number of polar groups on the surface, which greatly increases its adsorption capacity for methylene blue. Titanium dioxide distributed on the surface of biochar has a good photocatalytic effect on the adsorbed methylene blue, accelerating the degradation of methylene blue.

[0024] Economic aspect: The service life of biocarbon-based composite photocatalytic materials is much longer than that of pure biochar, which reduces the input cost of biochar and maximizes production economy. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of the peanut shell biochar-based titanium dioxide composite photocatalyst prepared in Example 1 of the present invention;

[0026] Figure 2 FT-IR comparison of peanut shells, biochar and biochar after phosphoric acid activation. DETAILED DESCRIPTION

[0027] The present invention provides a method for preparing a biochar-based titanium dioxide composite photocatalyst, comprising the following steps:

[0028] 1) mixing peanut shell particles, titanium dioxide and sodium lauryl sulfate to obtain a mixture;

[0029] 2) The mixture is activated and calcined in sequence to obtain a biochar-based titanium dioxide composite photocatalyst.

[0030] In the present invention, the particle size of the peanut shell particles is 200-300 mesh, preferably 200 mesh.

[0031] In the present invention, the mass ratio of the peanut shell particles, titanium dioxide and sodium dodecyl sulfate is 1-3: 0.05-0.2: 0.1-0.3, preferably 1.5-2.5: 0.08-1.5: 0.15-0.25, and more preferably 2: 0.1: 0.2.

[0032] In the present invention, the mixture is dried at 40-60° C. for 1-3 hours to a loose state before the activation treatment, preferably at 50° C. for 2 hours to a loose state.

[0033] In the present invention, in step 2), a phosphoric acid solution is used as an activating agent for activation treatment, and the concentration of the phosphoric acid solution is 80-90wt%, preferably 82-88wt%, and more preferably 85wt%.

[0034] In the present invention, the temperature of the activation treatment is 20-30° C., preferably 25° C.; the time of the activation treatment is 0.5-2 h, preferably 1 h.

[0035] In the present invention, the activation treatment is carried out under stirring.

[0036] In the present invention, in step 2), the mass volume ratio of the mixture to the phosphoric acid solution is 1-3.5 g: 3-10 mL, preferably 1.5-3 g: 4-8 mL, and more preferably 2-2.5 g: 5 mL.

[0037] In the present invention, after the mixture is activated, it is dried by forced air at 40-60° C. for 1-3 h, preferably at 50° C. for 2 h.

[0038] In the present invention, in the step 2), the calcination treatment is carried out under a protective atmosphere, and the protective atmosphere contains nitrogen and / or argon, preferably nitrogen.

[0039] In the present invention, the calcination temperature is 400-500°C, preferably 420-480°C, and more preferably 450°C; the calcination time is 0.5-2h, preferably 1.0-1.5h, and more preferably 1h; the heating rate of the calcination is 8-12°C / min, preferably 9-11°C / min, and more preferably 10°C / min.

[0040] The invention provides a biochar-based titanium dioxide composite photocatalyst.

[0041] The invention provides an application of a biochar-based titanium dioxide composite photocatalyst in photocatalytic degradation of organic pollutants.

[0042] In the present invention, the specific method for photocatalytic degradation of organic pollutants is: adding biochar-based titanium dioxide composite photocatalyst into organic wastewater, and catalyzing the reaction under the irradiation of cold light xenon lamp.

[0043] In the present invention, the concentration of methylene blue in the organic wastewater is 10-20 mg / L, preferably 15 mg / L.

[0044] In the present invention, the content of the biochar-based titanium dioxide composite photocatalyst in the organic wastewater is 0.1-1 g / L, preferably 0.2-0.9 g / L, and more preferably 0.3-0.8 g / L.

[0045] In the present invention, the distance between the cold light xenon lamp and the organic wastewater is 18-22 cm, preferably 20 cm, and the irradiation time is 0.5-2 h, preferably 0.8-1.5 h, and more preferably 1 h.

[0046] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention. Example 1

[0047] The precursor of biochar, peanut shell, was crushed and sieved, and a 200-mesh sieve was used to remove dust, soil and other impurities, and then the material was placed at 50°C for air drying until constant weight. 2.0g peanut shell particles, 0.2g sodium dodecyl sulfate, 0.1g titanium oxide, and 5mL 85wt% phosphoric acid solution were placed in a beaker for activation reaction and stirred for 1h. The above mixture was dried in an oven at 50°C for 2h until it was loose. Then it was placed in a nitrogen atmosphere of a tubular furnace roasting tube, and the temperature was raised to 450°C at a heating rate of 10°C / min and maintained at this temperature for 1h. The obtained product was washed with deionized water until the washed solution was neutral, dried to constant weight, ground to a relatively dispersed state, and packed into a plastic bag for use, which was recorded as catalyst 1. Take 0.02g of catalyst 1 and add it to 50mL of methylene blue solution (10mg / L). Control the power of the cold light source xenon lamp to 80w. Place the container on a magnetic stirrer 20cm away from the beaker containing the methylene blue solution wastewater. Stir at a speed of 300r / min. The reaction lasts for 40min, during which samples are taken and analyzed every 10min. Example 2

[0048] The precursor of biochar, peanut shell, was crushed and sieved, and a 200-mesh sieve was used to remove dust, soil and other impurities, and then the material was placed at 50°C for air drying until constant weight. 2.5g peanut shell particles, 0.3g sodium dodecyl sulfate, 0.15g titanium oxide, and 8mL 85wt% phosphoric acid solution were placed in a beaker for activation reaction and stirred for 1h. The above mixture was dried in an oven at 50°C for 2h until it was loose. Then it was placed in a nitrogen atmosphere of a tubular furnace roasting tube, and the temperature was raised to 500°C at a heating rate of 10°C / min and maintained at this temperature for 1h. The obtained product was washed with deionized water until the washed solution was neutral, dried to constant weight, ground to a relatively dispersed state, and packed into a plastic bag for use, which was recorded as catalyst 2. Take 0.04g of catalyst 2 and add it to 50mL of methylene blue solution (10mg / L). Control the power of the cold light source xenon lamp to 80w. Place the container on a magnetic stirrer 20cm away from the beaker containing the methylene blue solution wastewater. Stir at a speed of 300r / min. The reaction lasts for 40min, during which samples are taken and analyzed every 10min. Example 3

[0049] The precursor of biochar, peanut shell, was crushed and sieved, and a 200-mesh sieve was used to remove dust, soil and other impurities, and then the material was placed at 50°C for air drying until constant weight. 1.5g peanut shell particles, 0.3g sodium dodecyl sulfate, 0.05g titanium oxide, and 5mL 80wt% phosphoric acid solution were placed in a beaker for activation reaction and stirred for 1h. The above mixture was dried in an oven at 50°C for 2h until it was loose. Then it was placed in a nitrogen atmosphere of a tubular furnace roasting tube, and the temperature was raised to 480°C at a heating rate of 12°C / min and maintained at this temperature for 1h. The obtained product was washed with deionized water until the washed solution was neutral, dried to constant weight, ground to a relatively dispersed state, and packed into a plastic bag for use, which was recorded as catalyst 3. Take 0.02g of catalyst 3 and add it to 50mL of methylene blue solution (10mg / L). Control the power of the cold light source xenon lamp to 80w. Place the container on a magnetic stirrer 20cm away from the beaker containing the methylene blue solution wastewater and stir at a speed of 300r / min. The reaction lasts for 40min, during which samples are taken and analyzed every 10min. Comparative Example 1

[0050] The precursor of biochar, peanut shell, was crushed and sieved, and a 200-mesh sieve was used to remove dust, soil and other impurities, and then 2g of peanut shell particles were placed at 50°C for blast drying until constant weight. Then it was placed in a nitrogen atmosphere of a tubular furnace roasting tube, and the temperature was raised to 450°C at a heating rate of 10°C / min and maintained at this temperature for 1h. The obtained product was washed with deionized water until the washed solution was neutral, dried to constant weight, ground to a relatively dispersed state, and packed into a plastic bag for standby use, which was recorded as biochar. Take 0.02g of biochar and add it to 50mL of methylene blue solution (10mg / L), control the power of the cold light source xenon lamp to 80w, and place it about 20cm away from the beaker containing the methylene blue solution wastewater. The container was placed on a magnetic stirrer and stirred at a speed of 300r / min. The reaction lasted for 40min, and samples were taken and analyzed every 10min during the reaction. Comparative Example 2

[0051] The precursor of biochar, peanut shell, was crushed and sieved, and a 200-mesh sieve was used to remove dust, soil and other impurities, and then the material was placed at 50°C for air drying until constant weight. 2.0g peanut shell particles, 0.1g titanium dioxide, and 5mL 85wt% phosphoric acid solution were placed in a beaker and mixed evenly, and stirred for 1h. The above mixture was dried in an oven at 50°C for 2h until it was loose. Then it was placed in a nitrogen atmosphere of a tubular furnace roasting tube, and the temperature was raised to 450°C at a heating rate of 10°C / min and maintained at this temperature for 1h. The obtained product was washed with deionized water until the washed solution was neutral, dried to constant weight, ground to a relatively dispersed state, and packed into a plastic bag for use, which was recorded as catalyst 4. Take 0.02g of catalyst 4 and add it to 50mL of methylene blue solution (10mg / L). Control the power of the cold light source xenon lamp to 80w. Place the container on a magnetic stirrer about 20cm away from the beaker containing the methylene blue solution wastewater. Stir at a speed of 300r / min. The reaction lasts for 40min, during which samples are taken and analyzed every 10min. Comparative Example 3

[0052] First, the peanut shells, the precursor of biochar, were crushed and sieved, and a 200-mesh sieve was used to remove dust, soil and other impurities, and then the material was placed at 50°C for air drying until constant weight. 2.0g peanut shell particles, 0.2g sodium dodecyl sulfate, and 5mL 85wt% phosphoric acid solution were placed in a beaker and mixed evenly, and stirred for 1h. The above mixture was dried in an oven at 50°C for 2h until it was loose. Then it was placed in a nitrogen atmosphere in a tubular furnace roasting tube, and the temperature was raised to 450°C at a heating rate of 10°C / min and maintained at this temperature for 1h. The obtained product was washed with deionized water until the washed solution was neutral, dried to constant weight, ground to a relatively dispersed state, and packed into a plastic bag for use, which was recorded as catalyst 5. Take 0.02g of catalyst 5 and add it to 50mL of 10mg / L methylene blue solution. Control the power of the cold light source xenon lamp to 80w. Place the container on a magnetic stirrer at a distance of about 20cm from the beaker containing the methylene blue solution wastewater. Stir at a speed of 300r / min. The reaction lasts for 40min, during which samples are taken and analyzed every 10min.

[0053] The degradation effects of the catalysts obtained in Examples 1 to 3 and Comparative Examples 1 to 3 on methylene blue in organic wastewater are shown in Table 1 below:

[0054]

[0055] It can be seen from the above embodiments that the present invention provides a biochar-based titanium dioxide composite photocatalyst and its preparation method and application. The experimental results show that the composite catalyst modified by comprehensive activation of phosphoric acid, sodium dodecyl sulfate and titanium dioxide performs well in the removal and degradation of methylene blue dye, and has an efficient and rapid treatment effect. Compared with biochar prepared separately, the composite catalyst prepared by the method of the present invention has a fast degradation onset and high degradation efficiency. Under the condition of the same concentration of catalyst, the degradation efficiency of methylene blue in the simulated wastewater can reach up to 97.09% after 40 minutes. After catalyst 1 is repeatedly recycled three times, the last removal efficiency of methylene blue in the simulated wastewater can still reach 76.23%.

[0056] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a biochar-based titanium dioxide composite photocatalyst, characterized in that: The following steps are involved: 1) mixing peanut shell particles, titanium dioxide and sodium lauryl sulfate to obtain a mixture; 2) The mixture is activated and calcined in sequence to obtain a biochar-based titanium dioxide composite photocatalyst; The particle size of the peanut shell particles is 200-300 meshes, and the mass ratio of the peanut shell particles, titanium dioxide and sodium dodecyl sulfate is 1-3: 0.05-0.2: 0.1-0.3; In the step 2), a phosphoric acid solution is used as an activating agent for the activation treatment, and the concentration of the phosphoric acid solution is 80-90 wt %.

2. The preparation method according to claim 1, characterized in that: The temperature of the activation treatment is 20-30° C., and the time of the activation treatment is 0.5-2 h.

3. The preparation method according to claim 1 or 2, characterized in that: In the step 2), the mass volume ratio of the mixture to the phosphoric acid solution is 1-3.5 g: 3-10 mL.

4. The preparation method according to claim 1 or 2, characterized in that: In the step 2), the calcination treatment is performed under a protective atmosphere, and the protective atmosphere contains nitrogen and / or argon.

5. The preparation method according to claim 4, characterized in that: The temperature of the calcination treatment is 400-500° C., the time of the calcination treatment is 0.5-2 hours, and the heating rate of the calcination treatment is 8-12° C. / min.

6. The biochar-based titanium dioxide composite photocatalyst obtained by the preparation method according to any one of claims 1 to 5.

7. Use of the biochar-based titanium dioxide composite photocatalyst described in claim 6 in photocatalytic degradation of organic pollutants.

Citation Information

Patent Citations

  • Titanium dioxide / active carbon photocatalyst and preparation method and application thereof

    CN103240069A

  • Iron and nitrogen co-doping titanium dioxide / active carbon photocatalyst

    CN103240110A

  • Preparation method of walnut shell-based biomass carbon visible light-induced photocatalyst

    CN109985636A

  • Carboxymethyl magnetic lignin-based biochar and preparation method thereof

    CN111203196A

  • Silicon-rich biomass-based biochar / mesoporous silica composite material as well as preparation method and application thereof

    CN112675814A