A method for removing chromium and titanium from ammonium metavanadate using a reducing agent

By modifying aluminum powder and graphene-loaded reducing agents to reduce chromium and titanium in ammonium metavanadate under ultrasonic conditions, combined with filtration and recrystallization technology, it is solved that chromium and titanium in ammonium metavanadate are difficult to remove in ammonium metavanadate in the prior art. The problem of this paper realizes the preparation and stability of high-purity ammonium metavanadate and improves production efficiency.

CN116282152BActive Publication Date: 2024-11-05HUNAN ZHONGXIN NEW MATERIALS TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310300111.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-26
Publication Date
2024-11-05
Estimated Expiration
2043-03-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove chromium and titanium from ammonium metavanadate, which affects product quality, and the existing methods are complex in operation, making it difficult to achieve high-purity ammonium metavanadate preparation.

Method used

Using modified aluminum powder and graphene-supported reducing agents, mixing and reaction under ultrasonic conditions, chromium and titanium in ammonium metavanadate are selectively reduced to produce corresponding compounds, and high purity metamorphism is achieved through filtration and recrystallization. Ammonium vanadate preparation.

Benefits of technology

The high purity (≥99.9%) preparation of ammonium metavanadate was achieved, and the content of chromium and titanium was reduced to <5ppm, which improved the purity and production efficiency of the product, and ensured the stability and high purity of ammonium metavanadate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A method for removing chromium and titanium from ammonium metavanadate using a reducing agent comprises the following steps: (1) preparing modified aluminum powder; (2) preparing a reducing agent: mixing modified aluminum powder, sodium sulfite, and ammonium chloride in a mass ratio of 1:0.01-0.05:0.01-0.05, adding graphene equivalent to 10-20% of the mass of the modified aluminum powder, and mixing under ultrasonic conditions to obtain a modified aluminum powder loaded with reducing agent graphene; (3) dissolving the raw material ammonium metavanadate in hot water, adding a reducing agent, reacting for more than 30 minutes until no precipitation is produced, the reaction is terminated, filtering, and taking a filtrate; (4) recrystallization. The purity of the ammonium metavanadate obtained by the present invention is ≥99.9%, wherein the content of chromium is <5ppm, and the content of titanium is <5ppm. The ammonium metavanadate product obtained by the present invention has stable quality and high production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical industry, and particularly relates to a method for removing chromium and titanium from ammonium metavanadate by utilizing a reducing agent. Background Art

[0002] Ammonium metavanadate, molecular formula is NH 4 VO 3 , white or slightly yellowish crystalline powder, relative density 2.326, molecular weight 116.98, slightly soluble in cold water, hot ethanol and ether, soluble in hot water and dilute ammonium hydroxide. It turns into vanadium pentoxide when burned in the air.

[0003] Ammonium metavanadate is an intermediate product of vanadium refining. It is mainly used to produce vanadium pentoxide (powder or flake), and then further produce metallic vanadium, ferrovanadium alloy or other vanadium-based alloys. It can also be used as a chemical reagent, catalyst, drying agent, mordant, etc. It is widely used as a glaze in the ceramic industry. With the wide application of ammonium metavanadate in various industries, the requirements for the purity of ammonium metavanadate are getting higher and higher.

[0004] When high-purity ammonium metavanadate is used to prepare vanadium pentoxide or used in vanadium electrolyte, chromium and titanium elements have a great influence on product quality. Therefore, a method for removing chromium and titanium from ammonium metavanadate is urgently needed. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for removing chromium and titanium from ammonium metavanadate by using a reducing agent. The method is relatively simple to operate and the obtained ammonium metavanadate has high purity.

[0006] The technical solution adopted by the present invention to solve the technical problem is a method for removing chromium and titanium from ammonium metavanadate by using a reducing agent, comprising the following steps:

[0007] (1) Preparation of modified aluminum powder: mixing aluminum powder with benzenesulfonic acid equivalent to 1-3% of the weight of the aluminum powder, and dispersing under ultrasonic conditions for more than 30 minutes to obtain modified aluminum powder;

[0008] Furthermore, in step (1), the frequency of ultrasound is 1.2 to 1.5 kHz, and the time of ultrasonic dispersion is 10 to 20 minutes. If the ultrasonic dispersion time is too short, the modified aluminum powder cannot be evenly dispersed, which easily causes the material to agglomerate and the modification effect is not good; if the dispersion time is too long, the morphology of the compound is easily damaged.

[0009] Aluminum powder has good reduction performance, but if it is not modified, it is very easy to react under acidic or alkaline conditions. Studies have shown that the use of benzenesulfonic acid to modify aluminum powder inhibits the reaction performance of aluminum powder under acidic or alkaline conditions, but when it is added to ammonium metavanadate in the subsequent reaction process, it can still maintain good selective reduction performance for elements such as chromium and titanium, and has good selectivity.

[0010] (2) preparing a reducing agent: mixing the modified aluminum powder obtained in step (1), sodium sulfite, and ammonium chloride in a mass ratio of 1:0.01-0.05:0.01-0.05, adding graphene equivalent to 10-20% of the mass of the modified aluminum powder, and mixing under ultrasonic conditions to obtain a modified aluminum powder loaded with reducing agent graphene;

[0011] Studies have shown that the modified aluminum powder loaded with graphene, a reducing agent prepared by adding sodium sulfite and ammonium chloride, has good selectivity for reducing chromium and titanium elements in ammonium metavanadate.

[0012] Furthermore, in step (2), the frequency of ultrasound is 1.5 to 1.8 kHz, and the time of ultrasonic mixing is 5 to 10 minutes. If the ultrasonic mixing time is too short, the graphene cannot be evenly dispersed, which may easily cause material agglomeration; if the ultrasonic mixing time is too long, the graphene morphology may be damaged.

[0013] (3) dissolving the raw material ammonium metavanadate in hot water (preferably 50-60° C.), adding the reducing agent graphene-loaded modified aluminum powder obtained in step (3), and reacting for more than 30 minutes until no precipitation is produced. When the reaction is completed, filtering, and collecting the filtrate;

[0014] The modified aluminum powder particles loaded with the reducing agent graphene prepared by the present invention have consistent morphology and are evenly dispersed, and have a high impurity element loading amount. After reducing the impurity ions, the impurity ions are further adsorbed, which is conducive to the adsorption of impurities, and the reduction and adsorption are completed in one step. Studies have shown that the present invention adds a reducing agent to the vanadium liquid to reduce hexavalent chromium and tetravalent titanium to trivalent chromium and divalent titanium, generate corresponding compounds, and enter the impurity slag through filtration, and harmful elements are removed, and the chromium and titanium impurity ions in ammonium metavanadate can be better removed, and the adsorption of ammonium metavanadate is less. Insoluble impurities such as graphene can be filtered out.

[0015] Furthermore, in step (3), the raw material ammonium metavanadate is ammonium metavanadate with a purity of ≥99%. It contains a certain amount of chromium and titanium. Generally speaking, the chromium content is <0.3%, and the titanium content is <0.3%. If the chromium and titanium content in the raw material ammonium metavanadate is too high and the purity of the ammonium metavanadate is too low, the crude ammonium metavanadate can be initially purified by other methods, and then the chromium and titanium can be removed by the method of the present invention.

[0016] Furthermore, in step (3), the mass ratio of the raw material ammonium metavanadate to hot water is 0.03-0.08:1.

[0017] (4) adding ammonium metavanadate crystals to the filtrate obtained in step (3) for recrystallization to obtain ammonium metavanadate precipitate, separating the solid from the liquid, and drying to obtain ammonium metavanadate.

[0018] In the step (4) of the present invention, by adding ammonium metavanadate seeds to destroy the supersaturation of the solution during vanadium precipitation, the vanadium precipitation time can be shortened, the contact time between ammonium metavanadate and impurities can be reduced, and the product purity of ammonium metavanadate can be improved without adversely affecting the product purity.

[0019] The purity of the ammonium metavanadate obtained by the invention is ≥99.9%, wherein the content of chromium is less than 5ppm, and the content of titanium is less than 5ppm. The ammonium metavanadate product obtained by the invention has stable quality and high production efficiency.

[0020] The invention purifies ammonium metavanadate, separates harmful elements such as chromium and titanium therein, adds a special reducing agent to reduce the chromium and titanium in the ammonium metavanadate to low-price, and then generates corresponding compounds, removes impurities after filtration to obtain a high-purity sodium metavanadate solution, and further recrystallizes to obtain high-purity ammonium metavanadate. DETAILED DESCRIPTION

[0021] The present invention is further described in detail below in conjunction with specific embodiments. Example 1

[0022] The method of removing chromium and titanium from ammonium metavanadate by using a reducing agent in this embodiment comprises the following steps:

[0023] (1) Preparation of modified aluminum powder: aluminum powder was mixed with benzenesulfonic acid equivalent to 1% of the weight of aluminum powder, and dispersed under ultrasonic conditions for 30 minutes to obtain modified aluminum powder;

[0024] In step (1), the frequency of ultrasound is 1.2-1.5 kHz, and the ultrasonic dispersion time is 20 minutes. If the ultrasonic dispersion time is too short, the modified aluminum powder cannot be evenly dispersed, which easily causes the material to agglomerate and the modification effect is not good; if the dispersion time is too long, the morphology of the compound is easily damaged.

[0025] Aluminum powder has good reduction performance, but if it is not modified, it is very easy to react under acidic or alkaline conditions. Studies have shown that the use of benzenesulfonic acid to modify aluminum powder inhibits the reaction performance of aluminum powder under acidic or alkaline conditions, but when it is added to ammonium metavanadate in the subsequent reaction process, it can still maintain good selective reduction performance for elements such as chromium and titanium, and has good selectivity.

[0026] (2) preparing a reducing agent: mixing the modified aluminum powder obtained in step (1), sodium sulfite and ammonium chloride in a mass ratio of 1:0.01:0.05, adding graphene equivalent to 10% of the mass of the modified aluminum powder, and mixing under ultrasonic conditions to obtain a modified aluminum powder loaded with reducing agent graphene;

[0027] Studies have shown that the modified aluminum powder loaded with graphene, a reducing agent prepared by adding sodium sulfite and ammonium chloride, has good selectivity for reducing chromium and titanium elements in ammonium metavanadate.

[0028] In step (2), the frequency of ultrasound is 1.5 to 1.8 kHz, and the ultrasonic mixing time is 10 minutes. If the ultrasonic mixing time is too short, the graphene cannot be evenly dispersed, which may easily cause material agglomeration; if the ultrasonic mixing time is too long, the graphene morphology may be damaged.

[0029] (3) dissolving the raw material ammonium metavanadate in hot water at 50° C., adding the reducing agent graphene-loaded modified aluminum powder obtained in step (3), and reacting for 30 minutes until no precipitation is produced. After the reaction is completed, filtering, and collecting the filtrate;

[0030] The modified aluminum powder particles loaded with the reducing agent graphene prepared by the present invention have consistent morphology and are evenly dispersed, and have a high impurity element loading amount. After reducing the impurity ions, the impurity ions are further adsorbed, which is conducive to the adsorption of impurities, and the reduction and adsorption are completed in one step. Studies have shown that the present invention adds a reducing agent to the vanadium liquid to reduce hexavalent chromium and tetravalent titanium to trivalent chromium and divalent titanium, generate corresponding compounds, and enter the impurity slag through filtration, and harmful elements are removed, and the chromium and titanium impurity ions in ammonium metavanadate can be better removed, and the adsorption of ammonium metavanadate is less. Insoluble impurities such as graphene can be filtered out.

[0031] In step (3), the raw material ammonium metavanadate is ammonium metavanadate with a purity of 99%, wherein the content of chromium is 0.1% and the content of titanium is 0.2%. The mass ratio of the raw material ammonium metavanadate to hot water is 0.03:1.

[0032] (4) adding ammonium metavanadate crystals to the filtrate obtained in step (3) for recrystallization to obtain ammonium metavanadate precipitate, separating the solid from the liquid, and drying to obtain ammonium metavanadate.

[0033] In the step (4) of the present invention, by adding ammonium metavanadate seeds to destroy the supersaturation of the solution during vanadium precipitation, the vanadium precipitation time can be shortened, the contact time between ammonium metavanadate and impurities can be reduced, and the product purity of ammonium metavanadate can be improved without adversely affecting the product purity.

[0034] The purity of the ammonium metavanadate obtained in this embodiment is 99.95%, wherein the content of chromium is 4 ppm and the content of titanium is 3 ppm. The ammonium metavanadate product obtained by the present invention has stable quality and high production efficiency.

[0035] In this embodiment, ammonium metavanadate is purified to separate harmful elements such as chromium and titanium, and a special reducing agent is added to reduce the chromium and titanium in the ammonium metavanadate to low-price levels, and then corresponding compounds are generated. After filtration and impurity removal, a high-purity sodium metavanadate solution is obtained, and further recrystallization is performed to obtain high-purity ammonium metavanadate. Example 2

[0036] The method of removing chromium and titanium from ammonium metavanadate by using a reducing agent in this embodiment comprises the following steps:

[0037] (1) Preparation of modified aluminum powder: aluminum powder was mixed with benzenesulfonic acid equivalent to 2% of the weight of aluminum powder, and dispersed under ultrasonic conditions for 40 minutes to obtain modified aluminum powder;

[0038] In step (1), the frequency of ultrasound is 1.2-1.5 kHz, and the ultrasonic dispersion time is 15 minutes. If the ultrasonic dispersion time is too short, the modified aluminum powder cannot be evenly dispersed, which easily causes the material to agglomerate and the modification effect is not good; if the dispersion time is too long, the morphology of the compound is easily damaged.

[0039] Aluminum powder has good reduction performance, but if it is not modified, it is very easy to react under acidic or alkaline conditions. Studies have shown that the use of benzenesulfonic acid to modify aluminum powder inhibits the reaction performance of aluminum powder under acidic or alkaline conditions, but when it is added to ammonium metavanadate in the subsequent reaction process, it can still maintain good selective reduction performance for elements such as chromium and titanium, and has good selectivity.

[0040] (2) preparing a reducing agent: mixing the modified aluminum powder obtained in step (1), sodium sulfite and ammonium chloride in a mass ratio of 1:0.03:0.02, adding graphene equivalent to 15% of the mass of the modified aluminum powder, and mixing under ultrasonic conditions to obtain a modified aluminum powder loaded with reducing agent graphene;

[0041] Studies have shown that the modified aluminum powder loaded with graphene, a reducing agent prepared by adding sodium sulfite and ammonium chloride, has good selectivity for reducing chromium and titanium elements in ammonium metavanadate.

[0042] In step (2), the frequency of ultrasound is 1.5 to 1.8 kHz, and the ultrasonic mixing time is 10 minutes. If the ultrasonic mixing time is too short, the graphene cannot be evenly dispersed, which may easily cause material agglomeration; if the ultrasonic mixing time is too long, the graphene morphology may be damaged.

[0043] (3) dissolving the raw material ammonium metavanadate in hot water at 55° C., adding the reducing agent graphene-loaded modified aluminum powder obtained in step (3), reacting for 35 minutes until no precipitation is produced, filtering and collecting the filtrate after the reaction is completed;

[0044] The modified aluminum powder particles loaded with the reducing agent graphene prepared by the present invention have consistent morphology and are evenly dispersed, and have a high impurity element loading amount. After reducing the impurity ions, the impurity ions are further adsorbed, which is conducive to the adsorption of impurities, and the reduction and adsorption are completed in one step. Studies have shown that the present invention adds a reducing agent to the vanadium liquid to reduce hexavalent chromium and tetravalent titanium to trivalent chromium and divalent titanium, generate corresponding compounds, and enter the impurity slag through filtration, and harmful elements are removed, and the chromium and titanium impurity ions in ammonium metavanadate can be better removed, and the adsorption of ammonium metavanadate is less. Insoluble impurities such as graphene can be filtered out.

[0045] In step (3), the raw material ammonium metavanadate is ammonium metavanadate with a purity of 99%, wherein the chromium content is 0.2% and the titanium content is 0.1%. The mass ratio of the raw material ammonium metavanadate to hot water is 0.05:1.

[0046] (4) adding ammonium metavanadate crystals to the filtrate obtained in step (3) for recrystallization to obtain ammonium metavanadate precipitate, separating the solid from the liquid, and drying to obtain ammonium metavanadate.

[0047] In the step (4) of the present invention, by adding ammonium metavanadate seeds to destroy the supersaturation of the solution during vanadium precipitation, the vanadium precipitation time can be shortened, the contact time between ammonium metavanadate and impurities can be reduced, and the product purity of ammonium metavanadate can be improved without adversely affecting the product purity.

[0048] The purity of the ammonium metavanadate obtained in this embodiment is 99.91%, wherein the content of chromium is 2ppm and the content of titanium is 4ppm. The ammonium metavanadate product obtained by the present invention has stable quality and high production efficiency.

[0049] In this embodiment, ammonium metavanadate is purified to separate harmful elements such as chromium and titanium, and a special reducing agent is added to reduce the chromium and titanium in the ammonium metavanadate to low-price levels, and then corresponding compounds are generated. After filtration and impurity removal, a high-purity sodium metavanadate solution is obtained, and further recrystallization is performed to obtain high-purity ammonium metavanadate. Example 3

[0050] The method of removing chromium and titanium from ammonium metavanadate by using a reducing agent in this embodiment comprises the following steps:

[0051] (1) Preparation of modified aluminum powder: aluminum powder was mixed with benzenesulfonic acid equivalent to 3% of the weight of aluminum powder, and dispersed under ultrasonic conditions for 60 minutes to obtain modified aluminum powder;

[0052] In step (1), the frequency of ultrasound is 1.2-1.5 kHz, and the ultrasonic dispersion time is 20 minutes. If the ultrasonic dispersion time is too short, the modified aluminum powder cannot be evenly dispersed, which easily causes the material to agglomerate and the modification effect is not good; if the dispersion time is too long, the morphology of the compound is easily damaged.

[0053] Aluminum powder has good reduction performance, but if it is not modified, it is very easy to react under acidic or alkaline conditions. Studies have shown that the use of benzenesulfonic acid to modify aluminum powder inhibits the reaction performance of aluminum powder under acidic or alkaline conditions, but when it is added to ammonium metavanadate in the subsequent reaction process, it can still maintain good selective reduction performance for elements such as chromium and titanium, and has good selectivity.

[0054] (2) preparing a reducing agent: mixing the modified aluminum powder obtained in step (1), sodium sulfite and ammonium chloride in a mass ratio of 1:0.05:0.01, adding graphene equivalent to 20% of the mass of the modified aluminum powder, and mixing under ultrasonic conditions to obtain a modified aluminum powder loaded with reducing agent graphene;

[0055] Studies have shown that the modified aluminum powder loaded with graphene, a reducing agent prepared by adding sodium sulfite and ammonium chloride, has good selectivity for reducing chromium and titanium elements in ammonium metavanadate.

[0056] In step (2), the frequency of ultrasound is 1.5 to 1.8 kHz, and the ultrasonic mixing time is 10 minutes. If the ultrasonic mixing time is too short, the graphene cannot be evenly dispersed, which may easily cause material agglomeration; if the ultrasonic mixing time is too long, the graphene morphology may be damaged.

[0057] (3) dissolving the raw material ammonium metavanadate in hot water at 60° C., adding the reducing agent graphene-loaded modified aluminum powder obtained in step (3), and reacting for 50 minutes until no precipitation is produced. After the reaction is completed, filtering, and collecting the filtrate;

[0058] The modified aluminum powder particles loaded with the reducing agent graphene prepared by the present invention have consistent morphology and are evenly dispersed, and have a high impurity element loading amount. After reducing the impurity ions, the impurity ions are further adsorbed, which is conducive to the adsorption of impurities, and the reduction and adsorption are completed in one step. Studies have shown that the present invention adds a reducing agent to the vanadium liquid to reduce hexavalent chromium and tetravalent titanium to trivalent chromium and divalent titanium, generate corresponding compounds, and enter the impurity slag through filtration, and harmful elements are removed, and the chromium and titanium impurity ions in ammonium metavanadate can be better removed, and the adsorption of ammonium metavanadate is less. Insoluble impurities such as graphene can be filtered out.

[0059] In step (3), the raw material ammonium metavanadate is ammonium metavanadate with a purity of 99%, wherein the content of chromium is 0.1%, and the content of titanium is 0.1%. The mass ratio of the raw material ammonium metavanadate to hot water is 0.08:1.

[0060] (4) adding ammonium metavanadate crystals to the filtrate obtained in step (3) for recrystallization to obtain ammonium metavanadate precipitate, separating the solid from the liquid, and drying to obtain ammonium metavanadate.

[0061] In the step (4) of the present invention, by adding ammonium metavanadate seeds to destroy the supersaturation of the solution during vanadium precipitation, the vanadium precipitation time can be shortened, the contact time between ammonium metavanadate and impurities can be reduced, and the product purity of ammonium metavanadate can be improved without adversely affecting the product purity.

[0062] The purity of the ammonium metavanadate obtained in this embodiment is 99.90%, wherein the content of chromium is 4 ppm and the content of titanium is 3 ppm. The ammonium metavanadate product obtained by the present invention has stable quality and high production efficiency.

[0063] In this embodiment, ammonium metavanadate is purified to separate harmful elements such as chromium and titanium, and a special reducing agent is added to reduce the chromium and titanium in the ammonium metavanadate to low-price levels, and then corresponding compounds are generated. After filtration and impurity removal, a high-purity sodium metavanadate solution is obtained, and further recrystallization is performed to obtain high-purity ammonium metavanadate.

[0064] Comparative Example 1

[0065] In this comparative example, except that the aluminum powder is not modified with benzenesulfonic acid, other operations are exactly the same as those in Example 1. The purity of the ammonium metavanadate obtained in this comparative example is 99.51%, the chromium content is 0.05%, and the titanium content is 0.1%.

[0066] Comparative Example 2

[0067] In this comparative example, in step (1), ordinary mixing is used instead of ultrasonic dispersion, and other operations are exactly the same as those in Example 1. The purity of the ammonium metavanadate obtained in this comparative example is 99.62%, wherein the chromium content is 0.03% and the titanium content is 0.05%.

[0068] Comparative Example 3

[0069] In this comparative example, in step (2), sodium sulfite was not added, and the other operations were exactly the same as those in Example 1. The purity of the ammonium metavanadate obtained in this comparative example was 99.52%, wherein the chromium content was 0.04%, and the titanium content was 0.08%.

[0070] Comparative Example 4

[0071] In this comparative example, in step (2), ammonium chloride was not added, and the other operations were exactly the same as those in Example 1. The purity of the ammonium metavanadate obtained in this comparative example was 99.65%, wherein the chromium content was 0.03%, and the titanium content was 0.06%.

[0072] Comparative Example 5

[0073] In this comparative example, in step (2), graphene was not added, and the other operations were exactly the same as those in Example 1. The purity of the ammonium metavanadate obtained in this comparative example was 99.26%, wherein the chromium content was 0.08%, and the titanium content was 0.15%.

Claims

1. A method for removing chromium and titanium from ammonium metavanadate using a reducing agent, characterized in that: The following steps are involved: (1) Preparation of modified aluminum powder: mixing aluminum powder with benzenesulfonic acid equivalent to 1-3% of the weight of the aluminum powder, and dispersing under ultrasonic conditions for more than 30 minutes to obtain modified aluminum powder; (2) preparing a reducing agent: mixing the modified aluminum powder obtained in step (1), sodium sulfite, and ammonium chloride in a mass ratio of 1:0.01-0.05:0.01-0.05, adding graphene equivalent to 10-20% of the mass of the modified aluminum powder, and mixing under ultrasonic conditions to obtain a modified aluminum powder loaded with reducing agent graphene; (3) dissolving the raw material ammonium metavanadate in hot water, adding the reducing agent graphene-loaded modified aluminum powder obtained in step (2), reacting for more than 30 minutes until no precipitation is produced, filtering and collecting the filtrate after the reaction is completed; (4) adding ammonium metavanadate crystals to the filtrate obtained in step (3) for recrystallization to obtain ammonium metavanadate precipitate, separating the solid from the liquid, and drying to obtain ammonium metavanadate.

2. The method for removing chromium and titanium from ammonium metavanadate by using a reducing agent according to claim 1, characterized in that: In step (1), the frequency of ultrasound is 1.2 to 1.5 kHz.

3. The method for removing chromium and titanium from ammonium metavanadate by using a reducing agent according to claim 1 or 2, characterized in that: In step (1), the ultrasonic dispersion time is 10 to 20 minutes.

4. The method for removing chromium and titanium from ammonium metavanadate using a reducing agent according to claim 1 or 2, characterized in that: In step (2), the frequency of ultrasound is 1.5 to 1.8 kHz.

5. The method for removing chromium and titanium from ammonium metavanadate by using a reducing agent according to claim 1 or 2, characterized in that: In step (2), the ultrasonic mixing time is 5 to 10 minutes.

6. The method for removing chromium and titanium from ammonium metavanadate using a reducing agent according to claim 1 or 2, characterized in that: In step (3), the temperature of the hot water is 50-60°C.

7. The method for removing chromium and titanium from ammonium metavanadate using a reducing agent according to claim 1 or 2, characterized in that: In step (3), the mass ratio of the raw material ammonium metavanadate to hot water is 0.03-0.08:1.