A method for preparing a self-foaming directional macroporous bone cement scaffold

By preparing magnetic microspheres in calcium phosphate bone cement and controlling their movement using external magnetic field, the problem of difficult control of pore direction and size in calcium phosphate bone cement is solved, and a directional macroporous structure is formed, which promotes the growth and binding of bone tissue. strength.

CN116328034BActive Publication Date: 2024-11-22XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310365841.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-11-22
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

The existing calcium phosphate bone cement lacks a directional macroporous structure, resulting in limited flow of nutrients and body fluids, and the existing foaming method is difficult to control the pore direction and size.

Method used

Magnetic microspheres are prepared and coated with magnesium coating on their surfaces. The reaction of calcium carbonate and citric acid is used to generate bubbles, and the movement of the microspheres is controlled in combination with an external magnetic field to form a directional macroporous structure.

Benefits of technology

A directional macroporous bone cement scaffold with adjustable pore size and direction is realized, which promotes the flow of nutrients and body fluids and improves cell growth and binding strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004166636280000101
    Figure BDA0004166636280000101
Patent Text Reader

Abstract

The present invention discloses a method for preparing a self-foaming directional macroporous bone cement scaffold, which specifically comprises the following steps: step 1, preparing dynamic microspheres; step 2, preparing modified dynamic microspheres; step 3, preparing semi-coated microspheres; step 4, constructing a precursor slurry; and step 5, constructing a directional pore scaffold. The direction of pore formation is controlled by an external magnetic field, and bubbles are generated by reacting calcium carbonate with citric acid to form a unilateral driving force to promote the movement of microspheres, thereby obtaining a directional macroporous bone cement scaffold with adjustable pore size and direction. While ensuring directional macropores, it also has larger pores, which is conducive to the flow of nutrients and body fluids, thereby promoting the growth of cells in the pores and forming a firm bond.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic materials, in particular to a method for preparing a self-foaming directional macroporous bone cement scaffold. Background Art

[0002] Bone defect repair and treatment has always been a difficult and important issue in human medicine, and the demand for bone defect repair materials is also increasing. Traditional bone repair methods mainly include autologous bone and allogeneic bone transplantation. Due to the limited supply of autologous bone, immune rejection of allogeneic bone, and the need for secondary surgery, there are still many problems in medicine that need to be solved.

[0003] With the development of biomaterials, artificial bone repair materials have attracted much attention. Calcium phosphate cements (CPCs) have the advantages of bioactivity, bone conductivity, injectability and plasticity, but they have certain problems in clinical application. The lack of macroporous structure prevents nutrients and body fluids from flowing, and the lack of macroporous structure limits the growth of bone tissue and angiogenesis. Porous calcium phosphate cements with appropriate macropore size and high porosity have become a hot spot in current bone cement research.

[0004] Among the many methods for producing porous structures, the foaming method is simple and time-saving, but its main disadvantage is that it is associated with the sudden release of gas in the body and the pores produced are mostly closed pores with irregular shapes. Therefore, it is necessary to provide a method for preparing bone cement scaffolds that takes into account both the pore size and the controllable pore direction to produce directional large pores.

[0005] Qi Xiaopeng (Qi Xiaopeng, Ye Jiandong, Wang Xiupeng, Wang Yingjun. Preparation and characterization of macroporous calcium phosphate cement scaffolds with oriented pore structure [J]. Journal of the Chinese Ceramic Society, 2007) prepared macroporous calcium phosphate cement scaffolds with oriented pore structure by freeze-shaping. The porous calcium phosphate cement has interconnected macropores that are consistent with the growth direction of ice crystals, and the size of the pores can be adjusted by changing the freezing parameters. However, the direction of the pores can only be controlled by the direction of ice crystal growth and cannot be flexibly adjusted.

[0006] Zhou Wei (Zhou Wei. Preparation of α-TCP bone cement / gelatin microsphere composite scaffold material and its drug loading research [D]. Tianjin University, 2009.) added gelatin microspheres to bone cement. After the gelatin microspheres degraded, a porous bone cement scaffold with through holes and hydroxyapatite as the hydration product was obtained. As the amount of gelatin microspheres added increased, the porosity of the scaffold material increased. However, the direction of the pores formed was random and the pore direction could not be accurately controlled. Summary of the invention

[0007] The present invention provides a method for preparing a self-foaming directional macroporous bone cement scaffold, which solves the problem that the existing calcium phosphate bone cement lacks directional macropores. After preparing magnetic microspheres, the surface is modified by calcium carbonate, and a magnesium coating is coated on one-half of the surface of the microspheres. The other half of the uncoated calcium carbonate reacts quickly with citric acid to generate bubbles, thereby forming a unidirectional driving force. During the bone cement injection and curing process, the magnetic field is used to induce the change of the movement direction of the microspheres, thereby forming a directional macroporous structure.

[0008] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a self-foaming directional macroporous bone cement scaffold, which specifically comprises the following steps:

[0009] Step 1: Preparation of dynamic microspheres

[0010] The ferrosoferric oxide and polylactic acid were mixed and the dynamic microspheres were prepared by the emulsion solvent evaporation method.

[0011] Step 2, preparation of modified dynamic microspheres

[0012] The power microspheres in step 1 are added to a calcium chloride solution, carbon dioxide is introduced, and a reaction coating is prepared on the surface of the microspheres using a modifier to obtain surface-modified microspheres;

[0013] Step 3, preparation of semi-coated microspheres

[0014] Using a magnetic field to control the monolayer arrangement of the surface-modified microspheres obtained in step 2, sputtering a magnesium coating on half of the surface of the surface-modified microspheres by sputtering to obtain semi-coated microspheres;

[0015] Step 4: Constructing the precursor slurry

[0016] The semi-coated microspheres obtained in step 3 are uniformly mixed with the bone cement solid phase powder by ball milling, and then mixed with the bone cement liquid phase to obtain a precursor slurry;

[0017] Step 5: Build the directional hole bracket

[0018] The precursor slurry obtained in step 4 is injected into the mold, and an external magnetic field is applied, and then solidified and cured in a constant temperature and humidity chamber to form a bone cement scaffold with a directional macroporous structure.

[0019] Preferably, in step 1, ferroferric oxide Fe3O4 is 0.1-0.15 g, polylactic acid is 0.5-0.75 g, and ferroferric oxide Fe3O4 and polylactic acid are ultrasonically vibrated in an ultrasonic cleaner for 1-2 min; polyvinyl alcohol PVA1.0-1.5 g and distilled water 50-75 mL are used as solvents, and stirred for 1-1.5 hours at a temperature of 95°C and a rotation speed of 300-350 r / min.

[0020] Preferably, in step 1, the centrifugal rate of the ultrasonic oscillation is 5000-5500 r / min, the centrifugal time is 5-10 min, the water bath is heated to 65-70° C., the speed is 400-450 r / min, the stirring time is 2-3 h, and the filtration and drying are performed for 20-24 h.

[0021] Preferably, in step 2, the solubility of the calcium chloride solution is 2-4 mol / L, the volume fraction of carbon dioxide is 10%-30%, the rate of introducing carbon dioxide is 0.5-0.7 L / min, and the temperature is 20-40°C.

[0022] Preferably, in step 2, the modifier is sodium hexametaphosphate with a volume fraction of 1%-3%; and ammonia water is used to adjust the pH of the modifier to between 8 and 9.

[0023] Preferably, in step 3, the magnetic field size is 0.38 T, a micro-sputtering device is used to sputter in a vertical direction of the glass slide for 10-15 minutes, and the collected surface-modified microspheres are dried in an oven at 60-65°C.

[0024] Preferably, in step 4, the ball milling speed is 250-300 r / min, and the time is 2.5-3 h; the bone cement solid phase is a mixture of tetracalcium phosphate TTCP and dihydrate calcium hydrogen phosphate DCPD, with a solid content of 25% to 40%, and the liquid phase is an aqueous solution;

[0025] Preferably, in step 5, the external magnetic field is a static magnetic field, the magnitude of the static magnetic field is 0.38 T, and the direction of the magnetic field is consistent with the direction of the desired oriented macropores; the constant temperature and humidity conditions are: temperature is 37°, and humidity is 100%.

[0026] Beneficial effects of the present invention:

[0027] The direction of pore formation is controlled by an external magnetic field, and bubbles are generated by the reaction of calcium carbonate and citric acid to form a unilateral driving force to promote the movement of microspheres, thereby obtaining a directional macroporous bone cement scaffold with adjustable pore size and direction. While ensuring directional macropores, it also has larger pores, which is beneficial to the flow of nutrients and body fluids, thereby promoting cell growth in the pores and forming a strong bond. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be described clearly and completely below.

[0029] The method for preparing a self-foaming directional macroporous bone cement scaffold of the present invention is specifically implemented according to the following steps:

[0030] Step 1: Preparation of dynamic microspheres

[0031] The ferrosoferric oxide and polylactic acid were mixed and the dynamic microspheres were prepared by the emulsion solvent evaporation method.

[0032] 0.1-0.15 g of ferroferric oxide (Fe3O4), 0.5-0.75 g of polylactic acid; ultrasonic oscillation in an ultrasonic cleaner for 1-2 minutes; 1.0-1.5 g of polyvinyl alcohol (PVA), 50-75 mL of distilled water, temperature of 95°C, rotation speed of 300-350 r / min, stirring for 1-1.5 hours.

[0033] The centrifugal speed is 5000-5500r / min, the centrifugal time is 5-10min, the water bath is heated to 65-70°C, the speed is 400-450r / min, the stirring time is 2-3h, and the filtration and drying are 20-24h.

[0034] Step 2, preparation of modified dynamic microspheres

[0035] The power microspheres in step 1 are added to a calcium chloride solution, carbon dioxide is introduced, and a reaction coating is prepared on the surface of the microspheres using a modifier to obtain surface-modified microspheres.

[0036] The solubility of the calcium chloride solution is 2-4 mol / L, the volume fraction of carbon dioxide is 10%-30%, the ventilation rate is 0.5-0.7 L / min, and the temperature is 20-40°C.

[0037] The modifier is sodium hexametaphosphate with a volume fraction of 1%-3%; the pH value is adjusted to between 8 and 9 by ammonia water.

[0038] Step 3, preparation of semi-coated microspheres

[0039] The monolayer arrangement of the surface-modified microspheres obtained in step 2 is controlled by a magnetic field, and a magnesium coating is sputtered on half of the surface of the surface-modified microspheres by a sputtering method to obtain semi-coated microspheres.

[0040] The magnetic field size was 0.38 T. A micro-sputtering device was used to sputter in the vertical direction of the glass slide for 10-15 min. The collected microspheres were dried in an oven at 60-65°C.

[0041] Step 4: Constructing the precursor slurry

[0042] The semi-coated microspheres obtained in step 3 are uniformly mixed with the bone cement solid phase powder by ball milling, and then mixed with the bone cement liquid phase to obtain a precursor slurry.

[0043] The ball milling speed is 250-300r / min, and the time is 2.5-3h; the solid phase of the bone cement is a mixture of tetracalcium phosphate TTCP and dihydrate calcium hydrogen phosphate DCPD, with a solid content of 25% to 40%, and the liquid phase is an aqueous solution;

[0044] Step 5: Build the directional hole bracket

[0045] The precursor slurry obtained in step 4 is injected into the mold, and an external magnetic field is applied, and then solidified and cured in a constant temperature and humidity chamber to form a bone cement scaffold with a directional macroporous structure.

[0046] The magnitude of the static magnetic field is 0.38 T, and the direction of the magnetic field is consistent with the direction of the desired oriented macropores; the constant temperature and humidity conditions are: temperature is 37°, and humidity is 100%.

[0047] The present invention aims at the problem that bone cement lacks large-sized directional open pores. The present invention is a method for preparing a fast self-foaming directional macroporous bone cement scaffold. The desired pore-forming direction is controlled by an external magnetic field, and bubbles are generated by reacting calcium carbonate with citric acid to form a unilateral driving force to promote the movement of microspheres, thereby obtaining a directional macroporous bone cement scaffold with adjustable pore size and direction. While ensuring that the pore direction is consistent with the desired direction, the pore size is large, and the formation of directional macropores is conducive to the flow of nutrients and body fluids, thereby promoting cell growth in the pores and forming a firm bond.

[0048] Example 1

[0049] Weigh 0.1g of ferroferric oxide (Fe3O4) and 0.5g of polylactic acid and ultrasonically vibrate them in an ultrasonic cleaner for 1min; add 1.0g of polyvinyl alcohol (PVA) and 50mL of distilled water and stir for 1 hour at a temperature of 85℃ and a speed of 300r / min. Then centrifuge for 5min in a centrifuge at a centrifugal speed of 5000r / min, then heat to 60℃ in a water bath, stir for 2h at a speed of 400r / min, filter and dry for 20h to obtain dynamic microspheres.

[0050] When the temperature is controlled at 20°C, the dynamic microspheres are added to a 2 mol / L calcium chloride solution, 10% carbon dioxide by volume is introduced at a rate of 0.5 L / min, 1% sodium hexametaphosphate is added, and ammonia water is added to adjust the pH to 8, and a reaction coating is prepared on the surface of the microspheres to obtain surface-modified microspheres.

[0051] Under a static magnetic field of 0.38 T, the surface-modified microspheres were arranged in a single layer and sputtered vertically on a glass slide for 10 min using a micro-sputtering device to coat half of the microsphere surface with a magnesium coating. The collected microspheres were dried in an oven at 60 °C to obtain semi-coated microspheres.

[0052] The obtained semi-coated microspheres and the solid phase powder of bone cement with a solid content of 25% were added into the aqueous solution, and the mixture was ball-milled for 2.5 hours on a ball mill with a rotation speed of 250 r / min to obtain a precursor slurry.

[0053] The precursor slurry is injected into the mold, and a static magnetic field of 0.38T with a horizontal angle of 0° is applied. It is then cured and maintained in a constant temperature and humidity chamber with a temperature of 37° and a humidity of 100% to form a bone cement scaffold with a directional macroporous structure.

[0054] Example 2

[0055] Weigh 0.12g of ferroferric oxide (Fe3O4) and 0.6g of polylactic acid and ultrasonically vibrate in an ultrasonic cleaner for 1.5min; add 1.20g of polyvinyl alcohol (PVA) and 60mL of distilled water and stir for 1.25 hours at a temperature of 90℃ and a speed of 300r / min. Then centrifuge for 7min in a centrifuge at a centrifugal speed of 5200r / min, then heat in a water bath to 60℃, stir for 2.5h at a speed of 400r / min, filter and dry for 20h to obtain dynamic microspheres.

[0056] When the temperature is controlled at 25°C, the dynamic microspheres are added to a 2.5 mol / L calcium chloride solution, 15% carbon dioxide by volume is introduced at a rate of 0.55 L / min, 1.5% sodium hexametaphosphate is added, and ammonia water is added to adjust the pH to 8.5, and a reaction coating is prepared on the surface of the microspheres to obtain surface-modified microspheres.

[0057] Under a static magnetic field of 0.38 T, the surface-modified microspheres were arranged in a single layer and sputtered vertically on a glass slide for 12 min using a micro-sputtering device. A magnesium coating was coated on half of the surface of the microspheres. The collected microspheres were dried in an oven at 60°C to obtain semi-coated microspheres.

[0058] The obtained semi-coated microspheres and the bone cement solid phase powder with a solid content of 30% were added into the aqueous solution, and the mixture was ball-milled for 2.5 hours on a ball mill with a rotation speed of 250 r / min to obtain a precursor slurry.

[0059] The precursor slurry is injected into the mold, and a static magnetic field of 0.38T with a horizontal angle of 30° is applied. It is then cured and maintained in a constant temperature and humidity chamber at a temperature of 37° and a humidity of 100% to form a bone cement scaffold with a directional macroporous structure.

[0060] Example 3

[0061] Weigh 0.14g of ferroferric oxide (Fe3O4) and 0.7g of polylactic acid and ultrasonically vibrate them in an ultrasonic cleaner for 1.5min; add 1.4g of polyvinyl alcohol (PVA) and 70mL of distilled water and stir for 1.2 hours at a temperature of 90℃ and a speed of 320r / min. Then centrifuge for 8min in a centrifuge at a centrifugal speed of 5300r / min, then heat to 65℃ in a water bath, stir for 2.5h at a speed of 430r / min, filter and dry for 24h to obtain dynamic microspheres.

[0062] When the temperature is controlled at 35°C, the dynamic microspheres are added to a 3 mol / L calcium chloride solution, 25% carbon dioxide by volume is introduced at a rate of 0.6 L / min, 2% sodium hexametaphosphate is added, and ammonia water is added to adjust the pH to 8.5, and a reaction coating is prepared on the surface of the microspheres to obtain surface-modified microspheres.

[0063] Under a static magnetic field of 0.38 T, the surface-modified microspheres were arranged in a single layer and sputtered vertically on a glass slide for 14 minutes using a micro-sputtering device. A magnesium coating was coated on half of the surface of the microspheres. The collected microspheres were dried in an oven at 65°C to obtain semi-coated microspheres.

[0064] The obtained semi-coated microspheres and the solid phase powder of bone cement with a solid content of 35% were added into the aqueous solution, and the mixture was ball-milled for 2.5 hours on a ball mill with a rotation speed of 270 r / min to obtain a precursor slurry.

[0065] The precursor slurry is injected into the mold, and a static magnetic field of 0.38T with a horizontal angle of 60° is applied. It is then cured and maintained in a constant temperature and humidity chamber with a temperature of 37° and a humidity of 100% to form a bone cement scaffold with a directional macroporous structure.

[0066] Example 4

[0067] Weigh 0.15g of ferroferric oxide (Fe3O4) and 0.75g of polylactic acid and ultrasonically vibrate them in an ultrasonic cleaner for 2 minutes; add 1.5g of polyvinyl alcohol (PVA) and 75mL of distilled water and stir for 1.5 hours at a temperature of 955℃ and a speed of 350r / min. Then centrifuge for 10 minutes in a centrifuge with a centrifugal speed of 5500r / min, then heat to 70℃ in a water bath, stir for 3 hours at a speed of 450r / min, filter and dry for 24 hours to obtain dynamic microspheres.

[0068] When the temperature is controlled at 40°C, the dynamic microspheres are added to a 4 mol / L calcium chloride solution, 30% carbon dioxide by volume is introduced at a rate of 0.7 L / min, 3% sodium hexametaphosphate is added, and ammonia water is added to adjust the pH to 9, and a reaction coating is prepared on the surface of the microspheres to obtain surface-modified microspheres.

[0069] Under a static magnetic field of 0.38 T, the surface-modified microspheres were arranged in a single layer and sputtered in a vertical direction on a glass slide for 15 minutes using a micro-sputtering device. A magnesium coating was coated on half of the surface of the microspheres. The collected microspheres were dried in an oven at 65°C to obtain semi-coated microspheres.

[0070] The obtained semi-coated microspheres and the solid phase powder of bone cement with a solid content of 40% were added into the aqueous solution, and the mixture was ball-milled for 3 hours on a ball mill at a rotation speed of 3000 r / min to obtain a precursor slurry.

[0071] The precursor slurry is injected into the mold, and a static magnetic field of 0.38T with a horizontal angle of 90° is applied. It is then cured and maintained in a constant temperature and humidity chamber with a temperature of 37° and a humidity of 100% to form a bone cement scaffold with a directional macroporous structure.

[0072] Table 1 shows the pore direction, porosity, and pore size range corresponding to the samples prepared in Examples 1 to 4. As can be seen from Table 1, the directional macroporous bone cement scaffold prepared by the present invention has a pore direction that is consistent with the direction of the applied magnetic field, and the porosity and pore size range can be adjusted according to the size of the prepared dynamic microspheres. As the size of the dynamic microspheres increases, the pore size increases, and the porosity increases.

[0073] Table 1 shows the pore direction, porosity, and pore size range corresponding to the samples prepared in Examples 1 to 4;

[0074]

[0075] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a self-foaming directional macroporous bone cement scaffold, characterized in that: It consists of the following steps: Step 1: Preparation of dynamic microspheres The ferrosoferric oxide and polylactic acid were mixed and the dynamic microspheres were prepared by the emulsion solvent evaporation method. Weigh 0.1-0.15g of ferroferric oxide and 0.5-0.75g of polylactic acid; ultrasonically vibrate in an ultrasonic cleaner for 1-2min; add 1.0-1.5g of polyvinyl alcohol and 50-75mL of distilled water, stir for 1-1.5 hours at a temperature of 95°C and a speed of 300-350r / min; then centrifuge in a centrifuge at a centrifugal speed of 5000-5500r / min for 5-10min, then heat in a water bath to 65-70°C, at a speed of 400-450r / min, stir for 2-3h, filter and dry for 20-24h to obtain dynamic microspheres; Step 2, preparation of modified dynamic microspheres The power microspheres in step 1 are added to a calcium chloride solution, carbon dioxide is introduced, and a reaction coating is prepared on the surface of the microspheres using a modifier to obtain surface-modified microspheres; The solubility of calcium chloride solution is 2-4 mol / L, the volume fraction of carbon dioxide is 10%-30%, the rate of carbon dioxide introduction is 0.5-0.7 L / min, and the temperature is 20-40°C; The modifier is sodium hexametaphosphate, with a volume fraction of 1%-3%; the pH of the modifier is adjusted to between 8 and 9 by ammonia water; Step 3, preparation of semi-coated microspheres Using a magnetic field to control the monolayer arrangement of the surface-modified microspheres obtained in step 2, sputtering a magnesium coating on half of the surface of the surface-modified microspheres by sputtering to obtain semi-coated microspheres; The magnetic field size was 0.38 T, and a micro-sputtering device was used to sputter in the vertical direction of the glass slide for 10-15 min. The collected surface-modified microspheres were dried in an oven at 60-65°C. Step 4: Constructing the precursor slurry The semi-coated microspheres obtained in step 3 are uniformly mixed with the bone cement solid phase powder by ball milling, and then mixed with the bone cement liquid phase to obtain a precursor slurry; The solid phase of bone cement is a mixture of tetracalcium phosphate (TTCP) and dibasic calcium phosphate (DCPD) with a solid content of 25% to 40%; Step 5: Build the directional hole bracket The precursor slurry obtained in step 4 is injected into the mold, and an external magnetic field is applied, and then solidified and cured in a constant temperature and humidity chamber to form a bone cement scaffold with a directional macroporous structure.

2. The method for preparing a self-foaming directional macroporous bone cement scaffold according to claim 1, characterized in that: In step 4, the ball milling speed is 250-300 r / min and the time is 2.5-3 h.

3. The method for preparing a self-foaming directional macroporous bone cement scaffold according to claim 1, characterized in that: In step 5, the external magnetic field is a static magnetic field, the magnitude of the static magnetic field is 0.38 T, and the direction of the magnetic field is consistent with the direction of the desired oriented macropores; the constant temperature and humidity conditions are: temperature is 37° and humidity is 100%.