A method and system for continuous and controllable production of silicone resin microspheres

By using a hollow structure porous filter membrane with a porous filter in the production of silicone resin microspheres for hydrolysis and polycondensation reaction, the problems of large equipment occupation and low production efficiency in the prior art are solved, and high-efficiency and low-energy consumption of silicone resin microspheres are achieved Continuous production.

CN116376021BActive Publication Date: 2024-11-12GUIZHOU ZHENGYE LONGTENG NEW MATERIAL DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310480137.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-12
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

The existing silicone resin microsphere production methods have problems such as large equipment occupying space, low production efficiency, large amount of wastewater, and the inability to achieve continuous and efficient production.

Method used

The hollow structure porous filter membrane in the porous filter is used to carry out hydrolysis and polycondensation reaction of silane monomer and catalyst. By controlling the pH value, temperature and catalyst concentration, the continuous production of silicone resin microspheres is achieved, reducing equipment demand and cleaning frequency.

Benefits of technology

The continuous and controllable production of silicone resin microspheres is achieved, production efficiency is improved, energy consumption and wastewater treatment costs are reduced, and production processes are simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116376021B_ABST
    Figure CN116376021B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of silicone resin microspheres, and specifically relates to a method and a production system for continuously and controllably producing silicone resin microspheres, the method comprising: (1) conveying a silane monomer and a mixed dispersion of deionized water to a porous filter membrane and a hollow part of a porous filter a to form a monodisperse uniform emulsion; (2) conveying a catalyst solution and a monodisperse uniform emulsion to a porous filter membrane and a hollow part of a porous filter b to obtain a silicone resin microsphere solution through a polycondensation reaction; (3) the silicone resin microsphere solution flows into a storage tank and is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The present invention produces silicone resin microspheres in a continuous pipeline conveying manner, has no reactor, does not require waiting time for hydrolysis and polymerization reaction, has low energy consumption, can produce silicone resin microspheres in a continuous and controllable manner, improves the production efficiency of silicone resin microspheres, and simplifies the production process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicone resin microspheres, and particularly relates to a method and a production system for continuously and controllably producing silicone resin microspheres. Background Art

[0002] Silicone resin microspheres are solid spheres with a three-dimensional network structure. Because they contain non-polar methyl groups on the surface and a three-dimensional network structure inside, they have excellent physical and chemical properties such as high and low temperature resistance, smoothness, hydrophobicity, electrical insulation, physiological inertness, high fluidity, and optical properties. They can be widely used in the modification of optical properties of transparent optical plastics, the anti-adhesion of coatings and inks, and the smoothness and matting of cosmetics.

[0003] At present, silicone resin microspheres are all synthesized using intermittent and kettle processes, which require a large number of reactors, emulsification kettles, storage tanks, etc. The equipment takes up a large amount of space. In addition, because the equipment and containers in each section involved in the intermittent method need to be frequently cleaned when the specifications and models change to ensure that the required specifications and models meet the requirements, a large amount of washing wastewater is generated. Therefore, the existing production method has the disadvantages of being time-consuming and labor-intensive, low in production efficiency, and high in wastewater output.

[0004] In order to realize the continuous production of organosilicon spherical particles, the patent with the authorization announcement number CN 106633117B uses raw material components including polysiloxane containing silicon-hydrogen bonds, polysiloxane containing unsaturated carbon-carbon bonds, catalyst containing platinum group metals, curing delay agent, water and emulsifier, etc., which are premixed in three premixing devices and then emulsified, and then heated and cured by a heater, and finally filtered continuously by a continuous filtering device to obtain microspheres; in the patent with the authorization announcement number CN103214674B, the high-temperature and high-pressure reactor is used to synthesize organosilicon resin microspheres by hydrolysis and polymerization to improve its production efficiency and simplify the production process. The above preparation methods do not really realize the continuous and efficient production of silicone resin microspheres from the perspective of synthesis. First, premixing and emulsification require a large number of devices and time to participate in premixing and emulsification, and heating and curing also require time. There is an interval time in the middle, and discontinuous production; second, the high-temperature and high-pressure reactor accelerates the reaction mode and improves the synthesis efficiency in a high-energy consumption manner. Because of its high-temperature and high-pressure reaction, its existence requires a high-quality reactor and a precise control reaction process.

[0005] The patent with publication number CN101768272A discloses a continuous production system and production method of alkyl silicone resin, wherein the solution of alkyl chlorosilane prepared in step 1) is fed into the bottom of the reaction tower through the pipe C equipped with a metering pump by the raw material tank A; at the same time, the ethanol solution is fed into the top of the reaction tower E through the pipe D equipped with a metering pump by the raw material tank B; and the reciprocating vibrating screen plate installed in the reaction tower E is turned on, and the solution of the alkyl chlorosilane is mixed with the ethanol solution by vibration to carry out a hydrolysis reaction. The reaction tower and the washing tower with reciprocating vibrating screen plates can make the reactants contact quickly and achieve a rapid reaction; the alkyl chlorosilane solution is dispersed into micron-sized liquid droplets through a liquid distributor and enters the reaction tower, which can increase the contact area between the alkyl chlorosilane solution and the ethanol solution and reduce the occurrence of the cross-linking reaction of the alkyl silanol; the fixed plate of the reaction tower is cooled with water to conduct the generated heat in time to avoid excessive polycondensation of silanol and the generation of gel. However, this scheme still needs to be washed and concentrated after hydrolysis and before polycondensation, and still cannot completely solve the problem of requiring large equipment. Although this scheme is for the production of silicone resin, it usually uses various mixtures of methyltrichlorosilane, dimethyldichlorosilane, phenyltrichlorosilane, diphenyldichlorosilane or methylphenyldichlorosilane, which are hydrolyzed at a relatively low temperature of 1 to 25°C in the presence of an organic solvent such as toluene to obtain an acidic hydrolyzate. The initial hydrolysis product is a mixture of cyclic, linear and cross-linked polymers, which usually also contains multiple hydroxyl groups. The hydrolyzate is washed with water to remove the acid, and the neutral initial polycondensate is thermally oxidized in the air or further polycondensed in the presence of a catalyst to finally form a highly cross-linked three-dimensional network structure. Therefore, it is impossible to produce a microsphere structure, and a reaction residence time is required, and it is impossible to achieve a flow-type hydrolysis and polycondensation. Summary of the invention

[0006] Aiming at the deficiencies of the prior art, the present invention provides a method and equipment for continuously and controllably producing silicone resin microspheres.

[0007] This is achieved specifically through the following technical solutions:

[0008] A method for continuously and controllably producing silicone resin microspheres comprises the following steps:

[0009] (1) delivering a silane monomer to a porous filter a, and delivering a deionized water mixed dispersion to a hollow portion of the porous filter a, the silane monomer is pressed into the hollow portion of the porous filter a through a porous filter membrane of the porous filter a, and undergoes a hydrolysis reaction with the aqueous phase to form a monodisperse uniform emulsion;

[0010] (2) transporting the catalyst solution to the porous filter b, and at the same time transporting the monodisperse uniform emulsion to the hollow part of the porous filter b, the catalyst solution is pressed into the hollow part of the porous filter b through the porous filter membrane of the porous filter b, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution;

[0011] (3) The silicone resin microsphere solution flows into a storage tank, and then the silicone resin microsphere solution in the storage tank is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder.

[0012] In step (1), the delivery flow rate of the silane monomer is 30 kg / h to 150 kg / h, and the delivery pressure is 0.1 MPa to 5 MPa.

[0013] The silane monomer is at least one of methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane and phenyltrimethoxysilane.

[0014] The porous filter membrane is selected from at least one of an alumina ceramic porous filter membrane, a zirconia ceramic porous filter membrane, and a titanium oxide ceramic porous filter membrane.

[0015] The average pore diameter of the porous filter membrane in the porous filter a is 50nm-1500nm, the membrane thickness is 10mm-30mm, the inner diameter of the hollow part is 10mm-40mm, and the length is 500mm-1500mm.

[0016] The deionized water mixed dispersion is a mixed dispersion of a surfactant and deionized water.

[0017] The surfactant is at least one of fatty alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, fatty alcohol ether sulfate, fatty alcohol ether carboxylate, and polyvinyl pyrrolidone.

[0018] The pH value of the deionized water mixed dispersion is 2-6.

[0019] The delivery flow rate of the deionized water mixed dispersion is 300kg / h to 1500kg / h, and the temperature is 25 to 45°C.

[0020] In step (2), the delivery flow rate of the catalyst solution is 5kg / h to 80kg / h, the delivery pressure is 0.05MPa to 2.5MPa, and the temperature is 25 to 45°C.

[0021] The porous filter b has a porous filtration membrane with an average pore diameter of 3000nm to 7000nm, a membrane thickness of 10mm to 30mm, an inner diameter of the hollow part of 20mm to 60mm, and a length of 500mm to 1500mm.

[0022] The catalyst solution is an alkaline catalyst solution;

[0023] Furthermore, the alkaline catalyst solution is one of an aqueous ammonia solution, an aqueous NaOH solution, and an aqueous KOH solution.

[0024] Furthermore, the mass percentage concentration of the NaOH aqueous solution and the KOH aqueous solution is 5% to 25%, and the mass percentage concentration of the ammonia aqueous solution is 3% to 15%.

[0025] The delivery rate of the monodisperse uniform emulsion is 300kg / h to 1500kg / h.

[0026] The present invention adopts a porous filter membrane with a hollow structure for mass transfer and heat transfer. During hydrolysis, a homogeneous emulsion is formed through the porous filter membrane, and the silane monomer is rapidly solvated by controlling the pH and temperature. During polycondensation, an alkaline catalyst is formed into a homogeneous dispersion, and the catalyst is rapidly gelled by controlling the catalyst concentration, temperature, etc. The gelation reaction and the control of the pore size of the porous filter membrane can greatly shorten the time of hydrolysis and polycondensation, thereby realizing continuous synthesis of silicone resin microspheres and continuous production.

[0027] The present invention takes into account that the flow directly affects the size of the microsphere particle size, and the delivery pressure can affect the dispersion effect of the porous filter membrane, especially the delivery pressure needs to match the pore size of the porous filter membrane, so the control of the delivery flow, pressure and catalyst concentration also realizes the controllable production of the microsphere particle size. Among them, the parameters such as the pore size of the porous filter membrane in the porous filter a and the inner diameter of the hollow part are strictly controlled. On the one hand, when the average pore diameter is less than 50nm, it will lead to the difficulty of making the porous filter membrane and the high performance requirements of the delivery pump, and when the average pore diameter is greater than 1500nm, it will lead to poor homogenous dispersion effect; strictly controlling the average diameter of the porous filter membrane in the porous filter b will affect the polycondensation reaction speed and the dispersion speed of the catalyst solution, which is conducive to controlling the progress of the reaction.

[0028] In a porous filter, parameters such as the inner diameter of the hollow part, the thickness of the porous filter membrane, and the length of the filter will affect the flow rate, thereby affecting the mixing uniformity, the material contact, and the manufacturing difficulty. The present invention utilizes the filter membrane in the porous filter to press the silane monomer or the alkaline catalyst into the water phase or the monodisperse uniform emulsion for hydrolysis or polycondensation reaction, and by reasonably controlling various parameters, there is no need for residence time, and flow-type production is achieved.

[0029] A production system for continuously and controllably producing silicone microspheres comprises a silane storage tank, a dispersion storage tank, a silicone microsphere storage tank, an alkaline catalyst storage tank, a porous filter A and a porous filter B; the silane storage tank is connected to a feed port of the porous filter A through a delivery pipe, the dispersion storage tank is connected to a hollow part of the porous filter A through a delivery pipe; the discharge port of the porous filter A is connected to a hollow part of the porous filter B through a delivery pipe; the alkaline catalyst storage tank is connected to a feed port of the porous filter B through a delivery pipe; and the silicone microsphere storage tank is connected to an end of the hollow part of the porous filter B through a delivery pipe.

[0030] A pressure delivery pump, a flow meter, and a valve are sequentially installed on the delivery pipe; a pressure gauge is installed on the delivery pipe between the silane storage tank and the feed port of the porous filter a; and a pressure gauge is installed on the delivery pipe between the alkaline catalyst storage tank and the feed port of the porous filter b.

[0031] The porous filter comprises an outer cylinder and a porous filter membrane arranged inside the outer cylinder. The interior of the porous filter membrane is a hollow structure. A feed inlet and a discharge outlet are also arranged on the outer cylinder.

[0032] Beneficial effects:

[0033] The present invention utilizes the characteristics of the porous filter membrane with a hollow structure to produce silicone resin microspheres in a continuous pipeline transportation manner, thereby achieving the purpose of two-step continuous, controllable, and low-energy production. Through strict process control, it has the advantages of high production efficiency, time and labor saving, low wastewater treatment cost, low equipment investment cost, etc., and there is no need to invest in equipment such as reactors and emulsification reactors, thereby greatly reducing the cleaning frequency and space occupancy of the reaction equipment and simplifying the production process. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A continuous production system diagram of an embodiment of the present invention;

[0035] Figure 2 is a schematic diagram of the structure of a porous filter;

[0036] Figure 3 This is a scanning electron microscope image of Example 1 of the present invention;

[0037] Figure 4 This is a scanning electron microscope image of Example 2 of the present invention;

[0038] Figure 5 This is a scanning electron microscope image of Example 3 of the present invention;

[0039] Figure 6 This is a scanning electron microscope image of Example 4 of the present invention;

[0040] Figure 7 This is a scanning electron microscope image of Example 5 of the present invention;

[0041] Figure 8 This is a scanning electron microscope image of Example 6 of the present invention.

[0042] In the figure, 1-silane storage tank, 2-dispersion storage tank, 3-silicone resin microsphere storage tank, 4-alkaline catalyst storage tank, 5-delivery pipe A, 6-delivery pipe B, 7-delivery pipe C, 8-delivery pipe D, 9-delivery pipe E, 10-delivery pipe H, 11-delivery pipe G, 12-flow meter A, 13-flow meter B, 14-flow meter C, 15-valve A, 16-valve B, 17-valve C, 18-valve D, 19-valve E, 20-pressure gauge A, 21-pressure gauge B, 22-porous filter a, 23-porous filter b, 24-pressure delivery pump A, 25-pressure delivery pump B, 26-pressure delivery pump C, 27-flow meter D, 28-porous filter membrane, 29-outer cylinder, 30-hollow part, 31-feed port, 32 discharge port. DETAILED DESCRIPTION

[0043] The specific embodiments of the present invention are further described in detail below, but the present invention is not limited to these embodiments, and any improvement or substitution based on the basic spirit of the present embodiment still falls within the scope of protection required by the claims of the present invention.

[0044] Example 1

[0045] A production system for continuously and controllably producing silicone resin microspheres Figure 1 As shown, it includes a silane storage tank 1, a dispersion storage tank 2, a silicone microsphere storage tank 3, an alkaline catalyst storage tank 4, a porous filter a22, and a porous filter b23; the silane storage tank 1 is connected to the feed port of the porous filter a22 through a delivery pipe A5, and the dispersion storage tank 2 is connected to the hollow part of the porous filter a22 through a delivery pipe B6; the discharge port of the porous filter a22 is connected to the hollow part of the porous filter b23 through a delivery pipe D8; the alkaline catalyst storage tank 4 is connected to the feed port of the porous filter b23 through a delivery pipe H10; the silicone microsphere storage tank 3 is connected to the hollow part of the porous filter b23 through a delivery pipe E9; the silane storage tank 1 is connected to the discharge port of the porous filter a22 through a delivery pipe C7; the alkaline catalyst storage tank 4 is connected to the discharge port of the porous filter b23 through a delivery pipe G11.

[0046] The delivery pipe A5 is sequentially installed with a pressure delivery pump A24, a flow meter A12, a valve B16 and a pressure gauge A20.

[0047] The delivery pipe B6 is sequentially installed with a pressure delivery pump B25, a flow meter B13 and a valve C17.

[0048] A valve A15 is installed on the delivery pipe C7.

[0049] The delivery pipe D8 is provided with valves E19, flow valve D27 in sequence.

[0050] The delivery pipe H10 is sequentially installed with a pressure delivery pump C26, a flow meter C14, a valve D18 and a pressure gauge B21.

[0051] The porous filter structure is as follows Figure 2 As shown, the porous filter a22 and the porous filter b23 both include an outer cylinder 29 and a porous filter membrane 28 arranged inside the outer cylinder 29. The interior of the porous filter membrane 28 is a hollow part 30. The outer cylinder 29 is also provided with a feed port 31 and a discharge port 32, respectively.

[0052] The porous filter membrane of the porous filter a22 is an alumina ceramic porous filter membrane with an average pore diameter of 200 nm and a membrane thickness of 25 mm; the inner diameter of the hollow part 30 is 15 mm; and the length of the porous filter a22 is 1350 mm.

[0053] The porous filter membrane of the porous filter b23 is a zirconia ceramic porous filter membrane with an average pore diameter of 4000 nm and a membrane thickness of 25 mm; the inner diameter of the hollow part 30 is 45 mm; and the length of the porous filter b23 is 1200 mm.

[0054] use Figure 1 The production system and Figure 2 The method for continuously and controllably producing silicone resin microspheres using a porous filter comprises the following steps:

[0055] (1) The methyltrimethoxysilane monomer in the silane storage tank 1 is pressed into the porous filter membrane of the porous filter a22 at a flow rate of 55 kg / h and a pressure of 2.5 MPa through the delivery pipe A5 driven by the pressure delivery pump A24, and at the same time, the deionized water mixed dispersion in the dispersion storage tank 2 is passed through the hollow part of the porous filter a22 at a flow rate of 400 kg / h through the delivery pipe B6 driven by the pressure delivery pump B25; the silane monomer is pressed into the hollow part of the porous filter a22 through the porous filter membrane of the porous filter a22 to form a monodisperse uniform emulsion with the water phase, and the silane monomer not pressed into the hollow part flows back into the silane storage tank 1 from the delivery pipe C7; the deionized water mixed dispersion is sodium dodecyl sulfate dissolved and dispersed in deionized water, and the pH value of the deionized water mixed dispersion is 5.5 and the temperature is 30°C;

[0056] (2) The sodium hydroxide solution with a concentration of 8% and a temperature of 35° C. in the alkaline catalyst storage tank 4 is pressed into the porous filter membrane of the porous filter b23 through the delivery pipe H10 and the pressure delivery pump C26 at a flow rate of 15 kg / h and a pressure of 0.45 MPa. At the same time, the monodisperse uniform emulsion passes through the delivery pipe D8 through the valve E19 to control the flow rate at 451 kg / h through the hollow part of the porous filter membrane of the porous filter b23; the sodium hydroxide solution is pressed into the hollow part of the porous filter b23 through the porous filter membrane of the porous filter b23, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution. The sodium hydroxide solution that is not pressed into the hollow part flows back into the alkaline catalyst storage tank 4 from the delivery pipe G11;

[0057] (3) The organic silicone resin microsphere solution flows into the silicone resin microsphere storage tank 3 through the delivery pipe E9. The organic silicone resin microsphere solution in the silicone resin microsphere storage tank 3 is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The average particle size of the silicone resin microsphere powder is 1.42 μm. Figure 3 shown.

[0058] Example 2

[0059] A production system for continuously and controllably producing silicone resin microspheres Figure 1 As shown, the porous filter structure is as follows Figure 2 As shown, same as Example 1;

[0060] The porous filter membrane of the porous filter a22 is a zirconia ceramic porous filter membrane, the average diameter of the membrane pores is 50nm, and the membrane thickness is 25mm; the inner diameter of the hollow part 30 is 35mm; the length of the porous filter a22 is 1450mm;

[0061] The porous filter membrane of the porous filter b23 is an alumina ceramic porous filter membrane, the average diameter of the membrane pores is 4000nm, and the membrane thickness is 25mm; the inner diameter of the hollow part 30 is 45mm; the length of the porous filter b23 is 1200mm;

[0062] use Figure 1 The production system and Figure 2 The method for continuously and controllably producing silicone resin microspheres using a porous filter comprises the following steps:

[0063] (1) The methyltrimethoxysilane monomer in the silane storage tank 1 is pressed into the porous filter membrane of the porous filter a22 through the pipeline 5 at a flow rate of 35 kg / h and a pressure of 4.5 MPa under the drive of the pressure delivery pump A24. At the same time, the deionized water mixed dispersion in the storage tank 2 is passed through the pipeline 6 at a flow rate of 500 kg / h through the hollow part of the porous filter a22 under the drive of the pressure delivery pump B25. The silane monomer is pressed into the hollow part of the porous filter a22 through the porous filter membrane of the porous filter a22 to form a monodisperse uniform emulsion with the water phase. The silane monomer not pressed into the hollow part flows back into the silane storage tank 1 from the delivery pipe C7; the deionized water mixed dispersion is a mixture of fatty alcohol polyoxyethylene ether dissolved and dispersed in deionized water, and the pH value of the deionized water mixed dispersion is 4.5 and the temperature is 40°C;

[0064] (2) The sodium hydroxide solution with a concentration of 15% and a temperature of 45° C. in the alkaline catalyst storage tank 4 is pressed into the porous filter membrane of the porous filter b23 through the delivery pipe H10 via the pressure delivery pump C26 at a flow rate of 50 kg / h and a pressure of 1.5 MPa. At the same time, the monodisperse uniform emulsion passes through the delivery pipe D8 through the valve E19 to control the flow rate at 534 kg / h through the hollow part of the porous filter b23; the sodium hydroxide solution is pressed into the hollow part of the porous filter b23 through the porous filter membrane of the porous filter b23, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution. The sodium hydroxide solution that is not pressed into the hollow part flows back into the alkaline catalyst storage tank 4 from the delivery pipe G11;

[0065] (3) The organic silicone resin microsphere solution flows into the temporary silicone resin microsphere storage tank 3 through the delivery pipe E9. The organic silicone resin microsphere solution in the silicone resin microsphere storage tank 3 is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The average particle size of the silicone resin microsphere powder is 0.58 μm. Figure 4 shown.

[0066] Example 3

[0067] A production system for continuously and controllably producing silicone resin microspheres Figure 1 As shown, the porous filter structure is as follows Figure 2 As shown, same as Example 1;

[0068] The porous filter membrane of the porous filter a22 is an alumina ceramic porous filter membrane, the average diameter of the membrane pores is 850nm, and the membrane thickness is 15mm; the inner diameter of the hollow part 30 is 35mm; the length of the porous filter a22 is 1350mm;

[0069] The porous filter membrane of the porous filter b23 is a titanium oxide ceramic porous filter membrane, the average diameter of the membrane pores is 4500nm, and the membrane thickness is 25mm; the inner diameter of the hollow part 30 is 55mm; the length of the porous filter b23 is 1450mm;

[0070] use Figure 1 The production system and Figure 2 The method for continuously and controllably producing silicone resin microspheres using a porous filter comprises the following steps:

[0071] (1) The methyltrimethoxysilane monomer in the silane storage tank 1 is pressed into the porous filter membrane of the porous filter a22 through the pipeline 5 at a flow rate of 120 kg / h and a pressure of 3.5 MPa under the drive of the pressure delivery pump A24. At the same time, the deionized water mixed dispersion in the storage tank 2 is passed through the hollow part of the porous filter a22 through the pipeline 6 at a flow rate of 800 kg / h under the drive of the pressure delivery pump B25. The silane monomer is pressed into the hollow part of the porous filter a22 through the porous filter membrane of the porous filter a22 to form a monodisperse uniform emulsion with the water phase. The silane monomer not pressed into the hollow part flows back into the silane storage tank 1 from the delivery pipe C7; the deionized water mixed dispersion is prepared by dissolving and dispersing sodium dodecyl sulfate and fatty alcohol ether sulfate in deionized water, and the pH value of the deionized water mixed dispersion is 4.5 and the temperature is 26°C;

[0072] (2) The catalyst ammonia solution with a concentration of 4% and a temperature of 25° C. in the alkaline catalyst storage tank 4 is pressed into the porous filter membrane of the porous filter b23 through the delivery pipe H10 and the pressure delivery pump C26 at a flow rate of 20 kg / h and a pressure of 0.5 MPa. At the same time, the monodisperse uniform emulsion passes through the delivery pipe D8 through the valve E19 to control the flow rate at 918.5 kg / h through the hollow part of the porous filter b23. The ammonia solution is pressed into the hollow part of the porous filter b23 through the porous filter membrane of the porous filter b23, and undergoes a condensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution. The ammonia solution that is not pressed into the hollow part flows back into the alkaline catalyst storage tank 4 from the delivery pipe G11;

[0073] (3) The organic silicone resin microsphere solution flows into the temporary silicone resin microsphere storage tank 3 through the delivery pipe E9. The organic silicone resin microsphere solution in the silicone resin microsphere storage tank 3 is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The average particle size of the silicone resin microsphere powder is 6.5 μm. Figure 5 shown.

[0074] Example 4

[0075] A production system for continuously and controllably producing silicone resin microspheres Figure 1 As shown, the porous filter structure is as follows Figure 2As shown, same as Example 1;

[0076] The porous filter membrane of the porous filter a22 is a titanium oxide ceramic porous filter membrane, the average diameter of the membrane pores is 250nm, and the membrane thickness is 20mm; the inner diameter of the hollow part 30 is 20mm; the length of the porous filter a22 is 1050mm;

[0077] The porous filter membrane of the porous filter b23 is an alumina ceramic porous filter membrane, the average diameter of the membrane pores is 3500nm, and the membrane thickness is 25mm; the inner diameter of the hollow part 30 is 40mm; the length of the porous filter b23 is 1450mm;

[0078] use Figure 1 The production system and Figure 2 The method for continuously and controllably producing silicone resin microspheres using a porous filter comprises the following steps:

[0079] (1) The phenyltrimethoxysilane and methyltrimethoxysilane mixed monomers in the silane storage tank 1 in a ratio of 1:4 are pressed into the porous filter membrane of the porous filter a22 through the pipeline 5 at a flow rate of 60 kg / h and a pressure of 2.8 MPa under the drive of the pressure delivery pump A24. At the same time, the deionized water mixed dispersion in the storage tank 2 is passed through the hollow part of the porous filter a22 through the pipeline 6 at a flow rate of 800 kg / h under the drive of the pressure delivery pump B25. The silane monomer is pressed into the hollow part of the porous filter a22 through the porous filter membrane of the porous filter a22 to form a monodisperse uniform emulsion with the water phase. The silane monomer that is not pressed into the hollow part flows back into the silane storage tank 1 from the delivery pipe C7; the deionized water mixed dispersion is prepared by dissolving and dispersing sodium dodecyl sulfate and polyvinyl pyrrolidone in deionized water, and the pH value of the deionized water mixed dispersion is 5.2 and the temperature is 32° C.;

[0080] (2) The potassium hydroxide solution with a concentration of 12% and a temperature of 35° C. in the alkaline catalyst storage tank 4 is pressed into the porous filter membrane of the porous filter b23 through the delivery pipe H10 via the pressure delivery pump C26 at a flow rate of 55 kg / h and a pressure of 0.85 MPa. At the same time, the monodisperse uniform emulsion passes through the delivery pipe D8 through the valve E19 to control the flow rate of 858 kg / h through the hollow part of the porous filter b23; the potassium hydroxide solution is pressed into the hollow part of the porous filter b23 through the porous filter membrane of the porous filter b23, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution. The potassium hydroxide solution that is not pressed into the hollow part flows back into the alkaline catalyst storage tank 4 from the delivery pipe G11;

[0081] (3) The organic silicone resin microsphere solution flows into the temporary silicone resin microsphere storage tank 3 through the delivery pipe E9. The organic silicone resin microsphere solution in the silicone resin microsphere storage tank 3 is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The average particle size of the silicone resin microsphere powder is 1.6 μm. Figure 6 shown.

[0082] Example 5

[0083] A production system for continuously and controllably producing silicone resin microspheres Figure 1 As shown, the porous filter structure is as follows Figure 2 As shown, same as Example 1;

[0084] The porous filter membrane of the porous filter a22 is an alumina ceramic porous filter membrane, the average diameter of the membrane pores is 950nm, and the membrane thickness is 15mm; the inner diameter of the hollow part 30 is 42mm; the length of the porous filter a22 is 950mm;

[0085] The porous filter membrane of the porous filter b23 is an alumina ceramic porous filter membrane, the average diameter of the membrane pores is 5000nm, and the membrane thickness is 25mm; the inner diameter of the hollow part 30 is 55mm; the length of the porous filter b23 is 1450mm;

[0086] use Figure 1 The production system and Figure 2 The method for continuously and controllably producing silicone resin microspheres using a porous filter comprises the following steps:

[0087] (1) The vinyl trimethoxysilane monomer in the silane storage tank 1 is pressed into the porous filter membrane of the porous filter a22 through the pipeline 5 at a flow rate of 140 kg / h and a pressure of 1.8 MPa under the drive of the pressure delivery pump A24. At the same time, the deionized water mixed dispersion in the storage tank 2 is passed through the hollow part of the porous filter a22 through the pipeline 6 at a flow rate of 600 kg / h under the drive of the pressure delivery pump B25. The silane monomer is pressed into the hollow part of the porous filter a22 through the porous filter membrane of the porous filter a22 to form a monodisperse uniform emulsion with the water phase. The silane monomer that is not pressed into the hollow part flows back into the silane storage tank 1 from the delivery pipe C7; the deionized water mixed dispersion is a mixture of fatty alcohol ether carboxylate and polyvinyl pyrrolidone dissolved and dispersed in deionized water, and the pH value of the deionized water mixed dispersion is 4.3 and the temperature is 27°C;

[0088] (2) The ammonia solution with a concentration of 3.5% and a temperature of 32° C. in the alkaline catalyst storage tank 4 is pressed into the porous filter membrane of the porous filter b23 through the delivery pipe H10 and the pressure delivery pump C26 at a flow rate of 35 kg / h and a pressure of 0.15 MPa. At the same time, the monodisperse uniform emulsion passes through the delivery pipe D8 through the valve E19 to control the flow rate of 739 kg / h through the hollow part of the porous filter b23; the ammonia solution is pressed into the hollow part of the porous filter b23 through the porous filter membrane of the porous filter b23, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution. The sodium hydroxide solution that is not pressed into the hollow part flows back into the alkaline catalyst storage tank 4 from the delivery pipe G11;

[0089] (3) The organic silicone resin microsphere solution flows into the temporary silicone resin microsphere storage tank 3 through the delivery pipe E9. The organic silicone resin microsphere solution in the silicone resin microsphere storage tank 3 is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The average particle size of the silicone resin microsphere powder is 9.8 μm. Figure 7 shown.

[0090] Example 6

[0091] A production system for continuously and controllably producing silicone resin microspheres Figure 1 As shown, the porous filter structure is as follows Figure 2 As shown, same as Example 1;

[0092] The porous filter membrane of the porous filter a22 is a zirconia ceramic porous filter membrane, the average diameter of the membrane pores is 360nm, and the membrane thickness is 25mm; the inner diameter of the hollow part 30 is 28mm; the length of the porous filter a22 is 1000mm;

[0093] The porous filter membrane of the porous filter b23 is a zirconia ceramic porous filter membrane, the average diameter of the membrane pores is 3250nm, and the membrane thickness is 28mm; the inner diameter of the hollow part 30 is 36mm; the length of the porous filter b23 is 1350mm;

[0094] use Figure 1 The production system and Figure 2 The method for continuously and controllably producing silicone resin microspheres using a porous filter comprises the following steps:

[0095] (1) The ethyltrimethoxysilane monomer in the silane storage tank 1 is pressed into the porous filter membrane of the porous filter a22 through the pipeline 5 at a flow rate of 65 kg / h and a pressure of 2.2 MPa under the drive of the pressure delivery pump A24. At the same time, the deionized water mixed dispersion in the storage tank 2 is passed through the hollow part of the porous filter a22 through the pipeline 6 at a flow rate of 650 kg / h under the drive of the pressure delivery pump B25. The silane monomer is pressed into the hollow part of the porous filter a22 through the porous filter membrane of the porous filter a22 to form a monodisperse uniform emulsion with the water phase. The silane monomer not pressed into the hollow part flows back into the silane storage tank 1 from the delivery pipe C7; the deionized water mixed dispersion is sodium dodecylbenzene sulfonate dissolved and dispersed in deionized water, and the pH value of the deionized water mixed dispersion is 3.8 and the temperature is 31°C;

[0096] (2) The sodium hydroxide solution with a concentration of 12.5% ​​and a temperature of 33° C. in the alkaline catalyst storage tank 4 is pressed into the porous filter membrane of the porous filter b23 through the delivery pipe H10 via the pressure delivery pump C26 at a flow rate of 75 kg / h and a pressure of 0.95 MPa. At the same time, the monodisperse uniform emulsion passes through the delivery pipe D8 through the valve E19 to control the flow rate of 713 kg / h through the hollow part of the porous filter b23; the sodium hydroxide solution is pressed into the hollow part of the porous filter b23 through the porous filter membrane of the porous filter b23, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution. The sodium hydroxide solution that is not pressed into the hollow part flows back into the alkaline catalyst storage tank 4 from the delivery pipe G11;

[0097] (3) The organic silicone resin microsphere solution flows into the temporary silicone resin microsphere storage tank 3 through the delivery pipe E9. The organic silicone resin microsphere solution in the silicone resin microsphere storage tank 3 is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder. The average particle size of the silicone resin microsphere powder is 2.5 μm. Figure 8 shown.

Claims

1. A method for continuous and controllable production of silicone resin microspheres, characterized in that: The method comprises the following steps: (1) The silane monomer is transported to the porous filter a, and the deionized water mixed dispersion is transported to the hollow part of the porous filter a. The silane monomer is pressed into the hollow part of the porous filter a through the porous filter membrane of the porous filter a, and undergoes a hydrolysis reaction with the water phase to form a monodisperse uniform emulsion; The delivery flow rate of the silane monomer is 30kg / h~150kg / h, and the delivery pressure is 0.1MPa~5MPa; the silane monomer is at least one of methyltrimethoxysilane, ethyltrimethoxysilane, vinyltrimethoxysilane, and phenyltrimethoxysilane; The porous filter a has an average pore diameter of 50 nm to 1500 nm, a membrane thickness of 10 mm to 30 mm, an inner diameter of the hollow part of 10 mm to 40 mm, and a length of 500 mm to 1500 mm; The deionized water mixed dispersion is a mixed dispersion of a surfactant and deionized water; The surfactant is at least one of fatty alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, fatty alcohol ether sulfate, fatty alcohol ether carboxylate, and polyvinyl pyrrolidone; The pH value of the deionized water mixed dispersion is 2-6; the delivery flow rate of the deionized water mixed dispersion is 300kg / h-1500kg / h, and the temperature is 25-45°C; (2) The catalyst solution is transported to the porous filter b, and the monodisperse uniform emulsion is transported to the hollow part of the porous filter b. The catalyst solution is pressed into the hollow part of the porous filter b through the porous filter membrane of the porous filter b, and undergoes a polycondensation reaction with the monodisperse uniform emulsion to obtain a silicone resin microsphere solution; The delivery flow rate of the catalyst solution is 5kg / h~80kg / h, the delivery pressure is 0.05MPa~2.5MPa, and the temperature is 25~45°C; the catalyst solution is an alkaline catalyst solution; The porous filter membrane in the porous filter b has an average pore diameter of 3000nm to 7000nm, a membrane thickness of 10mm to 30mm, an inner diameter of the hollow part of 20mm to 60mm, and a length of 500mm to 1500mm; (3) The silicone resin microsphere solution flows into a storage tank, and then the silicone resin microsphere solution in the storage tank is filtered, washed, dried, and depolymerized to obtain silicone resin microsphere powder.

2. A method for continuously and controllably producing silicone resin microspheres as claimed in claim 1, characterized in that: The porous filter membrane is selected from at least one of an alumina ceramic porous filter membrane, a zirconia ceramic porous filter membrane, and a titanium oxide ceramic porous filter membrane.

3. A production system for continuous and controllable production of silicone resin microspheres, characterized in that: It is a production system for the method for continuously and controllably producing silicone resin microspheres as described in claim 1, specifically comprising a silane storage tank, a dispersion storage tank, a silicone resin microsphere storage tank, an alkaline catalyst storage tank, a porous filter a, and a porous filter b; the silane storage tank is connected to the feed port of the porous filter a through a delivery pipe, the dispersion storage tank is connected to the hollow part of the porous filter a through a delivery pipe; the discharge port of the porous filter a is connected to the hollow part of the porous filter b through a delivery pipe; the alkaline catalyst storage tank is connected to the feed port of the porous filter b through a delivery pipe; and the silicone resin microsphere storage tank is connected to the hollow end of the porous filter b through a delivery pipe.