A polylactic acid / citral electrospinning nanofiber membrane, preparation method and application thereof

The polylactic acid/citral nanofiber membrane prepared through electrospinning technology solves the problem of aquatic products. By sustained release of citral, it inhibits spoilage bacteria, extends shelf life and maintains the quality of aquatic products, and realizes the effectiveness of food preservation and environmental protection of fresh food sex.

CN116377653BActive Publication Date: 2024-11-15QINGDAO AGRI UNIV +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310384907.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-12
Publication Date
2024-11-15
Estimated Expiration
2043-04-12

AI Technical Summary

Technical Problem

Aquatic products have a high rate of corruption loss during storage, transportation and processing. Existing food preservation materials such as citral limit their application due to insoluble in water, easy oxidation and instability, and lack of effective refrigerated packaging materials to reduce the risk of corruption. .

Method used

Electrospinning technology is used to prepare polylactic acid/citral electrospinning nanofiber membranes. By combining citral as the core layer material with polylactic acid shell spinning liquid, nanofiber membranes are formed, and their high porosity and specific surface area are used. Sustained release, a mass sensing system wrapped on aquatic products to inhibit spoilage bacteria.

Benefits of technology

It effectively extends the shelf life of aquatic products, reduces the volatile salt-based nitrogen value and fat oxidation value, maintains the quality and freshness of aquatic products, and the materials are biodegradable and environmentally friendly, and have broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116377653B_ABST
    Figure CN116377653B_ABST
Patent Text Reader

Abstract

The invention discloses a polylactic acid / citral electrostatic spinning nanofiber membrane, a preparation method and application thereof, and belongs to the technical field of food preservative and fresh-keeping materials. The invention uses polylactic acid as a shell material, encapsulates citral, a quorum sensing inhibitor, and prepares a polylactic acid / citral coaxial spinning fiber membrane. The polylactic acid / citral electrostatic spinning nanofiber membrane of the invention has a smaller pore size, a higher specific surface area and porosity, a smooth surface, no other defects such as beads, has good hydrophobicity, thermal properties and mechanical properties, and also has a slow-release characteristic. The polylactic acid / citral electrostatic spinning nanofiber membrane of the invention can reduce the volatile basic nitrogen value and fat oxidation value of turbot during refrigeration, and has a good maintenance effect on the quality and freshness of turbot. Using it as a food packaging material is of great significance to improving the quality and shelf life of aquatic products, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of food preservative and fresh-keeping materials, and specifically relates to a polylactic acid / citral electrostatic spinning nanofiber membrane, a preparation method and application thereof. Background Art

[0002] Aquatic products are low in fat and high in protein, and are an important source of high-quality protein for humans, occupying a major position in the national diet and fishery economy. However, due to the immaturity of cold chain transportation technology, the corruption loss rate of aquatic products during storage, transportation, processing and sales is as high as 15%, causing huge economic losses and waste of resources.

[0003] Pseudomonas fluorescens is a specific spoilage bacterium for a variety of refrigerated aquatic products. Studies have shown that a variety of food spoilage-related characteristics of Pseudomonas fluorescens are regulated by its quorum sensing system. Therefore, interfering with its quorum sensing system may provide a possible way to eliminate bacterial resistance and extend the shelf life of aquatic products.

[0004] Citral has a strong quorum sensing inhibitory activity. Citral is a natural product that exists in lemongrass oil, lemon oil, lime oil, citrus oil, litsea cubeba oil, and verbena oil. It is also a food flavoring permitted by national regulations. It is mainly used to prepare lemon, citrus and assorted fruit flavors. It is also the main raw material for synthesizing ionones. However, citral is insoluble in glycerin and water, is easily oxidized, and is unstable, which reduces its bioavailability and limits its application in food preservation.

[0005] Electrospinning is a new technology that uses the breakdown effect of high-voltage electrostatic fields on polymer solutions to prepare nanofiber materials. The electrospinning process is simple and the conditions are mild. The prepared spinning fibers are small in size, with diameters ranging from a few nanometers to a few microns. They have the advantages of multiple functions, high porosity, and large specific surface area. Active substances can be embedded, which not only maintains the activity of the substances, but also enables the embedded active substances to be slowly released from the packaging material to the food surface. Summary of the invention

[0006] In view of the problems existing in the prior art, the object of the present invention is to provide a polylactic acid / citral electrospinning nanofiber membrane, a preparation method and application thereof.

[0007] In order to achieve the above object, the present invention adopts the following technical solution:

[0008] A polylactic acid / citral electrospinning nanofiber membrane, the preparation method is as follows:

[0009] The polylactic acid shell spinning solution and the citral core layer spinning solution were placed in syringes respectively, and the electrospinning parameters were set as follows: polylactic acid flow rate: 0.005-0.01 mm / min, citral flow rate: 0.2-0.4 mm / min; positive voltage was 24.58-26.76 kV, negative voltage was 1.64-1.83 kV; tin foil was used for receiving, the receiving distance was 15-20 cm, and the receiving time was 2-3 h, to obtain polylactic acid / citral electrospinning nanofiber membrane.

[0010] The electrospinning parameters of polylactic acid flow rate, citral flow rate, positive voltage, negative voltage, receiving distance and receiving time affect the uniformity, thickness and food preservation ability of the electrospinning membrane. Through experiments on the parameters of the electrospinning process, it was found that the increase of polylactic acid flow rate increased the shell thickness of the electrospinning membrane, which increased the release time of citral in the core layer material, so the polylactic acid flow rate was 0.005-0.01mm / min; the increase of citral flow rate led to an increase in the concentration of the core layer material, and the generated fibers showed more breakage phenomena, so the citral flow rate range was 0.2-0.4mm / min; during the spinning process, the voltage and receiving distance will also affect the spinning diameter. The greater the spinning voltage, the finer the diameter, the greater the spinning distance, and the larger the diameter of the spinning fiber. The spinning time directly affects the thickness of the spinning membrane. The longer the time, the greater the thickness. Taking into account the stability and freshness of the spinning membrane, the spinning parameters were determined as follows: positive voltage of 24.58-26.76 kV, negative voltage of 1.64-1.83 kV; tin foil was used for receiving, the receiving distance was 15-20 cm, and the receiving time was 2-3 h.

[0011] In a specific embodiment, the polylactic acid shell spinning solution is prepared by adding polylactic acid into a mixed solution of dichloromethane and DMF, stirring and dissolving, and then ultrasonicating.

[0012] In a specific embodiment, the power of the ultrasound is 0.1 W·cm -2 , frequency 50kHz, temperature 25℃.

[0013] In a specific embodiment, the concentration of the polylactic acid shell spinning solution is 9-12% by mass. The concentration of the polylactic acid shell spinning solution affects the diameter of the spinning membrane, thereby affecting the antiseptic and fresh-keeping effect on aquatic products. Polylactic acid solutions of different concentrations were spun, and it was found that with the increase of polylactic acid concentration, the viscosity of the spinning solution and the diameter of the spinning membrane increased. The increase in the viscosity of the spinning solution affects the spinnability of the fiber. Taking into account the spinnability and fresh-keeping performance of the spinning membrane, the concentration of polylactic acid in the polylactic acid shell spinning solution is selected to be 9-12% by mass for spinning.

[0014] The preparation method of the polylactic acid / citral electrospinning nanofiber membrane comprises the following steps:

[0015] Polylactic acid was added to a mixed solution of dichloromethane and DMF (volume ratio 1:1) and stirred to dissolve to obtain a polylactic acid solution with a mass fraction of 10%. The solution was magnetically stirred for 12 h and ultrasonicated for 2 h (ultrasonic power 0.1 W·cm -2 , ultrasonic frequency 50kHz, ultrasonic temperature 25℃), and then obtain the polylactic acid shell spinning solution. Citral is prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution, and the polylactic acid shell spinning solution and the citral core spinning solution are placed in syringes respectively. Electrospinning equipment: polylactic acid flow rate: 0.005mm / min, citral flow rate: 0.2mm / min; positive voltage is 24.58kV, negative voltage is 1.64kV, and tin foil is used for receiving, the receiving distance is 20cm, and the receiving time is 2h, and the polylactic acid / citral electrospinning nanofiber membrane is obtained.

[0016] The polylactic acid / citral electrospun nanofiber membrane prepared by the above method is used in food preservation and freshness preservation; wherein the food is aquatic products, such as turbot, sea cucumber, large yellow croaker, etc.

[0017] A method for preserving turbot fish meat, comprising: peeling the polylactic acid / citral electrospun nanofiber membrane prepared by the above method from tin foil, vacuum drying it, irradiating it under ultraviolet light for 15 minutes, using it to wrap turbot fish meat, and storing it at 0°C.

[0018] The polylactic acid / citral electrospinning nanofiber membrane prepared by the above method is used in the preparation of food packaging materials with antiseptic and fresh-keeping effects.

[0019] A food packaging material with antiseptic and fresh-keeping effects contains the polylactic acid / citral electrostatic spinning nanofiber film prepared by the above method.

[0020] Advantages of the technical solution of the present invention:

[0021] The present invention provides a novel refrigerated aquatic product packaging material by using electrostatic spinning technology, uses polylactic acid as a shell material, encapsulates citral, a quorum sensing inhibitor, prepares a polylactic acid / citral coaxial spinning fiber membrane, characterizes the prepared nanofiber membrane, and finds and tests its preservation effect on refrigerated turbot. The polylactic acid / citral electrostatic spinning nanofiber membrane of the present invention is of great significance to improving the quality and shelf life of aquatic products, and has broad application prospects.

[0022] The polylactic acid / citral electrospinning nanofiber membrane prepared by the electrospinning technology of the present invention has a smaller pore size, a higher specific surface area and porosity, a smooth surface, no other defects such as beads, good hydrophobicity, thermal properties and mechanical properties, and a slow-release characteristic. The polylactic acid / citral electrospinning nanofiber membrane of the present invention can reduce the volatile basic nitrogen value and fat oxidation value of turbot during refrigeration, and has a good effect on maintaining the quality and freshness of turbot.

[0023] In a kind of polylactic acid / citral electrostatic spinning nanofiber film of the present invention, the polylactic acid used is a biodegradable material, made using the starch raw material extracted from renewable plant resources, with good mechanical properties, physical properties, tensile strength, air permeability, oxygen permeability and carbon dioxide permeability and other characteristics, and polylactic acid can be completely degraded by microorganisms in nature, generating carbon dioxide and water, without polluting the environment, and is a recognized environmentally friendly material. And citral is a natural plant essential oil, a safe ingredient that can be added to food as specified by national standards, with insecticidal, anti-inflammatory, antioxidant, antifungal effects. Therefore a kind of polylactic acid / citral electrostatic spinning nanofiber film of the present invention, it is possible to realize the slow release of citral from packaging materials to the surface of aquatic products, and a good fresh-keeping effect is played to aquatic products such as turbot, with broad application prospects.

[0024] In conclusion, the present invention provides a reference for the future development and utilization of new food active packaging materials containing natural quorum sensing inhibitors. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a graph of the quorum sensing inhibitory activity of citral;

[0026] Figure 2 It is a scanning electron microscope image of electrospun nanofiber membrane (wherein, (a) polylactic acid / citral electrospinning; (b) polyethylene oxide / citral electrospinning; (c) zein / citral electrospinning; (d) polyethylene oxide + chitosan / citral electrospinning);

[0027] Figure 3 This is the infrared spectrum of polylactic acid / citral electrospun nanofiber membrane;

[0028] Figure 4 is the differential scanning calorimetry (DSC) graph of polylactic acid / citral electrospun nanofiber membrane;

[0029] Figure 5 is the X-ray diffraction pattern of polylactic acid / citral electrospun nanofiber membrane;

[0030] Figure 6 This is a test diagram of the mechanical properties of polylactic acid / citral electrospun nanofiber membrane;

[0031] Figure 7 is the sustained release behavior diagram of polylactic acid / citral electrospun nanofiber membrane;

[0032] Figure 8 This is a picture of the preservation effect of electrospun nanofiber membrane on turbot. DETAILED DESCRIPTION

[0033] The terms used in the present invention, unless otherwise specified, generally have the meanings commonly understood by those of ordinary skill in the art.

[0034] The present invention is further described in detail below in conjunction with specific examples and with reference to data. The following examples are only intended to illustrate the present invention and are not intended to limit the scope of the present invention in any way.

[0035] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.

[0036] In the following examples, strain C. violaceum CV026 was donated by Professor Li Jianrong of Bohai University and preserved in the laboratory of Special Food Research Institute of Qingdao Agricultural University.

[0037] Example 1 Inhibition of bacterial quorum sensing by citral

[0038] 1. Determination of minimum inhibitory concentration of citral

[0039] The minimum inhibitory concentration (MIC) of citral against C. violaceum CV026 was determined to ensure that the quorum sensing inhibitory activity of citral was due to its inhibition of the bacterial QS system rather than its antibacterial activity.

[0040] Here are the steps:

[0041] Citral was diluted with 70% methanol. 70% methanol and sterile water were used as blank controls. C. violaceum CV026 was cultured in a shaking incubator until OD 600 is 1.0. Then dilute it with LB broth at a ratio of 1:100. Add 100μL of bacterial solution to a 96-well plate, add 10μL of two-fold diluted citral in sequence, and incubate at 28°C for 24h. Use LB broth without citral as a blank control. Observe with the naked eye that the concentration of citral in the well with the lowest concentration in the 96-well plate with no bacterial growth is the MIC of citral. The minimum inhibitory concentration of citral is 1% (v / v), or 0.89mg / mL. Subsequent experiments were carried out at the sub-inhibitory concentration of citral.

[0042] 2. Inhibition of bacterial quorum sensing by citral

[0043] The reporter strain C. violaceum CV026 was cultured to OD 600 is 1.0. Add the culture to LB agar medium cooled to about 50℃ at a ratio of 1:100, mix well, pour into a plate (plate diameter 90mm) and punch holes with an Oxford cup. For C.violaceum CV026, 10μL of C6-HSL needs to be added to the LB agar. Add 100μL of sub-inhibitory citral to the wells of the plate, place in an incubator for 24h (28℃) and observe the color change of the plate.

[0044] The results showed that citral diluted to 1% (v / v) concentration did not show antibacterial activity against the reporter strain C. violaceum CV026. Figure 1 It can be seen that the C. violaceum CV026 plate is purple due to the presence of C6-HSL, which causes the reporter strain to produce violacein. When citral was injected, the purple substance around the wells decreased, indicating that citral has QS inhibitory activity and can inhibit short-chain signal molecules (AHLs).

[0045] Example 2

[0046] An electrospun nanofiber membrane, the preparation method is as follows:

[0047] Preparation of polylactic acid / citral electrospinning nanofiber membrane: polylactic acid was added to a mixed solution of dichloromethane and DMF (volume ratio 1:1) and stirred to dissolve to obtain a polylactic acid solution with a mass fraction of 10%. The solution was magnetically stirred for 12 h and ultrasonicated for 2 h (ultrasound power 0.1 W cm -2 , ultrasonic frequency 50kHz, ultrasonic temperature 25°C), to obtain polylactic acid shell spinning solution. Citral is prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution. The polylactic acid shell spinning solution and the core spinning solution are placed in syringes respectively. Electrospinning equipment: polylactic acid flow rate: 0.005mm / min, citral flow rate: 0.2mm / min. The positive voltage is 24.58kV, and the negative voltage is 1.64kV. Use tin foil for receiving, the receiving distance is 20cm, and the receiving time is 2h to obtain polylactic acid / citral electrospinning nanofiber membrane.

[0048] Comparative Example 1

[0049] An electrospun nanofiber membrane, the preparation method is as follows:

[0050] Preparation of polyethylene oxide / citral electrospinning nanofiber membrane: Polyethylene oxide (MW = 9 × 10 5) was dissolved in N,N-dimethylformamide solvent and stirred to dissolve to obtain a 7% polyethylene oxide solution; the solution was magnetically stirred for 12 h and ultrasonicated for 2 h (ultrasonic power 0.1 W·cm -2 , ultrasonic frequency 50kHz, ultrasonic temperature 25°C), to obtain ethylene oxide shell spinning solution. Citral is prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution. The ethylene oxide shell spinning solution and the core spinning solution are placed in syringes respectively. Electrospinning equipment: polyethylene oxide: 0.004mm / min, citral flow rate: 0.2mm / min. The positive voltage is 20.66kV, and the negative voltage is 1.37kV. Use tin foil for receiving, the receiving distance is 20cm, and the receiving time is 2h to obtain polyethylene oxide / citral electrospinning nanofiber membrane.

[0051] Comparative Example 2

[0052] An electrospun nanofiber membrane, the preparation method is as follows:

[0053] Preparation of zein / citral electrospinning nanofiber membrane: Zein was dissolved in 80% ethanol solution and stirred to dissolve, and a 30% zein solution was prepared. The solution was magnetically stirred for 12 h and ultrasonicated for 2 h (ultrasonic power 0.1 W·cm -2 , ultrasonic frequency 50kHz, ultrasonic temperature 25°C), the shell spinning solution of zein solution was obtained. Citral was prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution. The shell spinning solution and the core spinning solution of zein solution were placed in syringes respectively, and the electrospinning equipment was: zein: 0.005mm / min, citral flow rate: 0.2mm / min. The positive voltage was 18.61kV and the negative voltage was 2.94kV. It was received with tin foil, the receiving distance was 18cm, and the receiving time was 2h, and the zein / citral electrospinning nanofiber membrane was obtained.

[0054] Comparative Example 3

[0055] An electrospun nanofiber membrane, the preparation method is as follows:

[0056] Preparation of polyethylene oxide + chitosan / citral electrospinning nanofiber membrane: polyethylene oxide (MW = 9 × 10 5 ) and chitosan (MW = 1 × 10 6 ) were dissolved in 90% glacial acetic acid at a mass ratio of 9:1 to prepare a 5% polyethylene oxide + chitosan solution; the solution was magnetically stirred for 12 h and ultrasonically (ultrasound power 0.1 W cm -2, ultrasonic frequency 50kHz, ultrasonic temperature 25°C) for 2h to obtain polyethylene oxide + chitosan shell spinning solution. Citral is prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution. The polyethylene oxide + chitosan shell spinning solution and the core spinning solution are placed in syringes respectively, and the electrospinning equipment is: polyethylene oxide + chitosan: 0.004mm / min, citral flow rate: 0.2mm / min. The positive voltage is 19.54kV and the negative voltage is 2.82kV. Use tin foil for receiving, the receiving distance is 20cm, and the receiving time is 2h to obtain polyethylene oxide + chitosan / citral electrospinning nanofiber membrane.

[0057] Scanning electron microscopy observation of electrospun nanofiber membranes with different shell materials

[0058] The electrospun nanofiber membranes made of different shell materials prepared by the methods described in Example 2 and Comparative Examples 1-3 were observed using a scanning electron microscope. The electrospun nanofiber membranes made of different shell materials were cut into 3mm×3mm sizes, and after gold was sprayed on the surface, the surface structure of the fibers was observed using a scanning electron microscope.

[0059] The results are as follows Figure 2 As shown in the figure, by scanning electron microscopy observation of polylactic acid / citral electrospun nanofiber membrane, it was found that polylactic acid / citral electrospun nanofiber membrane had a smaller diameter, uniform thickness, fibers interlaced into a mesh, and a smooth surface, while nanofiber membranes made of citral wrapped with other materials had beads and other defects.

[0060] Characterization of polylactic acid / citral electrospun fiber membrane

[0061] 1. Near infrared spectroscopy detection: The polylactic acid / citral nanofiber membrane prepared in Example 2 was cut into pieces, fully ground with KBr, and then pressed into tablets using a tablet press. -1 The wavelength was measured by Fourier infrared spectroscopy.

[0062] The results are as follows Figure 3 As shown, (a) is uniaxial polylactic acid electrospinning at 1734.01 cm -1 A strong absorption peak appears at 1043.49cm, which is the -C=O stretching vibration peak; -1 , 1155.36cm -1 It is the characteristic absorption peak of ether bond (-CO- stretching vibration); 1435.04cm -1 , 1448.54cm -1 , 1467.83cm -1 It is the bending vibration of -CH3; 1328.95cm -1 , 1386.81cm -1(b) is the electrospinning of polylactic acid / citral. In addition to the characteristic peaks of polylactic acid, 1489.47 cm -1 The stretching vibration caused by the double bond of the benzene ring (C=C) is 2930.12 cm -1 It is the -CH2- stretching vibration absorption peak, which is a unique functional group of citral. The infrared spectrum data show that the chemical structure of polylactic acid and citral is not affected during the electrospinning process, and the two are mainly physically mixed.

[0063] 2. Thermal performance test:

[0064] 3 mg of the polylactic acid / citral electrospun nanofiber membrane prepared in Example 2 was cut into pieces and tested using a TG-DSC thermal analyzer; the results are shown in FIG. Figure 4 shown. Figure 4 (a) is uniaxial polylactic acid electrospinning. The initial decomposition temperature of uniaxial polylactic acid electrospinning is about 300℃, and the half decomposition temperature (T 50% ) is about 390℃. The pyrolysis temperature range of PLA spinning fiber is divided into two parts. The first part is 300-430℃, and the TG curve drops sharply. This is the first weight loss platform, and the weight loss rate is 89.3%; then there is the platform area of ​​the sample TG curve, which is also the thermal stability area of ​​the sample; the second part is 460-520℃, and the curve has a relatively gentle downward trend. This is the second weight loss platform, and the weight loss rate at this time is 7.3%. When the temperature rises to 520℃, the TG curve of the sample no longer changes, indicating that the quality of the sample tends to be stable after reaching this temperature, and the substance no longer decomposes. (b) is polylactic acid / citral electrospinning. It can be seen from the figure that the thermal decomposition curve of polylactic acid / citral spinning fiber is similar to that of polylactic acid spinning fiber, and also includes two pyrolysis processes. The initial decomposition temperature is about 270℃. The first weight loss platform appears in the range of 270~420℃. The TG curve drops sharply, and the weight loss rate is about 79.1%, followed by the platform area of ​​the curve. The temperature range of the second weight loss platform is 430~510℃, and the weight loss rate is about 14.6%. When the temperature is greater than 510℃, the curve no longer changes. The above results show that the polylactic acid material wrapped with citral has some effect on the thermal stability, but the overall trend of the curve does not change much. The DSC test of the spun fiber shows that the polylactic acid uniaxial spun fiber has an endothermic peak at about 65℃, which is the glass transition temperature (T g). A gentle endothermic peak appears near 110°C, but the corresponding TG curve shows no weight loss, so this temperature is the melting peak of the polylactic acid spun fiber. There are two obvious exothermic peaks at 390°C and 410°C, indicating that the sample decomposes at high temperature and generates a large amount of heat, corresponding to the first weight loss platform of the TG curve, and the sample has a large weight loss phenomenon; there is an obvious exothermic peak at 460°C, corresponding to the second weight loss platform of the TG curve, indicating that the sample further decomposes and releases heat. From the DSC curve of the polylactic acid / citral spun fiber, it can be seen that an endothermic peak appears at 88°C, which is the glass transition temperature (T g ). 190℃ is the melting temperature of polylactic acid / citral spinning fiber (T m ). g and T m The increase indicates that the addition of citral has an effect on the glass transition temperature and melting temperature of polylactic acid spinning fiber, that is, it affects its thermal properties. The polylactic acid / citral spinning fiber has an obvious exothermic peak at 400℃, indicating that the sample decomposes at this temperature and generates a lot of heat, corresponding to the first weight loss platform of the TG curve; there is an obvious exothermic peak at 465℃, and the sample further decomposes and releases heat at this temperature, corresponding to the second weight loss platform of the TG curve.

[0065] 3. X-ray diffraction detection

[0066] The polylactic acid / citral electrospun nanofiber membrane prepared in Example 2 was subjected to X-ray diffraction using an X-ray powder diffractometer; the results are as follows: Figure 5 shown. Figure 5 (a) is uniaxial electrospinning of polylactic acid, and (b) is electrospinning of polylactic acid / citral. The polylactic acid uniaxial electrospinning showed a broad diffraction peak at 2θ=21.60°, which is the characteristic diffraction peak of polylactic acid and shows crystalline characteristics. The crystallization peak of polylactic acid / citral electrospinning nanofiber membrane changed significantly and shifted greatly, indicating that the high voltage current had a great influence on the crystal structure of polylactic acid. The diffraction peak of polylactic acid / citral electrospinning nanofiber membrane was also broad, indicating that its crystallization effect was not good, which may also be the result of the mixing of crystalline and amorphous regions.

[0067] 4. Mechanical properties test

[0068] The polylactic acid / citral electrospun nanofiber membrane prepared in Example 2 was cut into a size of 70 mm×25 mm, and the tensile strength was tested using the tensile probe of a texture analyzer to calculate the tensile strength and elongation at break of the spun fiber.

[0069] Tensile strength: σt = P / (b×d).

[0070] σt: tensile strength, MPa; P is the tensile force when the sample breaks, N; b is the width of the sample, mm; d is the thickness of the sample, mm.

[0071] Elongation at break: εt = (L-L0) / L0×100%.

[0072] εt is the elongation at break; L0 is the original length of the sample, mm; L is the length of the sample when it breaks, mm.

[0073] Figure 6 The figure shows the mechanical properties of polylactic acid / citral electrospun nanofiber membranes. The tensile strength (σt) and elongation at break (εt) of polylactic acid / citral electrospun nanofiber membranes are calculated to be (1.348±0.031)MPa and (32.38±0.040)%, respectively. The polylactic acid / citral electrospun nanofiber membranes have good mechanical properties and tensile strength. The thickness of the fiber membrane is (0.0260±0.00127)mm, and the contact angle is (126.60±4.31)°, which is a hydrophobic material.

[0074] 5. Test on sustained release behavior of polylactic acid / citral electrospinning nanofiber membrane

[0075] Citral was prepared into solutions with different concentrations, and the absorbance was measured by ultraviolet spectrophotometer. The concentration and absorbance were linearly regressed to obtain the fitting equation.

[0076] 10 mg of the spun fiber prepared in Example 2 was accurately weighed, and 10 mL of PBS phosphate buffer (pH=7.4) was added. The mixture was oscillated at a constant temperature. Samples were taken regularly and the same amount of release medium was added. The absorbance value was measured, the drug concentration was calculated, and the release curve was drawn.

[0077] The results are as follows Figure 7 As shown by Figure 7 It can be seen that the free citral is released very quickly in the initial stage of release, with the release rate reaching 94.36% in 24 hours, and the release is slow in the later stage; while the polylactic acid / citral electrospinning nanofiber membrane has a sustained release behavior, and the encapsulated citral continues to be released over time without burst release behavior.

[0078] Example 3

[0079] Application of polylactic acid / citral electrospun nanofiber membrane in the preservation of turbot

[0080] Fresh turbot was purchased from the aquatic market, the head was stunned and then the skin was removed, and the turbot meat was sliced. The nanofiber membranes prepared in Example 2 and Comparative Examples 1, 2, and 3 were used to wrap turbot fillets, respectively, to determine their antiseptic and fresh-keeping effects on turbot. Different electrospun nanofiber membranes were peeled off from the tin foil, vacuum dried, and then irradiated under ultraviolet light for 15 minutes, and used to wrap turbot fillets, and turbot fillets not wrapped with spun fibers were used as the control group. The fish fillets of the control group and the test group were stored at 0°C, and the changes in the volatile basic nitrogen value and fat oxidation value of the control group and the test group were detected every 3 days.

[0081] 10g of precisely weighed turbot fish meat, MgO (1g), dH2O (50mL) and 3 drops of n-octanol were placed in a distillation tube, and the volatile basic nitrogen value was calculated using a FOSS Kjeldahl nitrogen analyzer; 10g of minced fish meat was added with 25mL of distilled water and 25mL of 10% trichloroacetic acid solution, and 5mL of supernatant was taken after homogenization and filtration, and 5mL of 0.02mol / L thiobarbituric acid solution was added, and the mixture was placed in a water bath at 80°C for 40min, and the absorbance was measured at 532nm after cooling. The 2-barbituric acid value was expressed as the mass fraction of malondialdehyde. The results are as follows Figure 8 shown.

[0082] Volatile basic nitrogen (TVB-N) is a kind of alkaline nitrogen-containing substances such as ammonia and amines produced by the decomposition of proteins by enzymes and bacteria during the spoilage process of food. It is the main indicator of the freshness of aquatic products. The results showed that the TVB-N of turbot fillets wrapped with and without electrospun nanofiber membranes increased with the extension of storage time. However, after being wrapped with polylactic acid / citral electrospun nanofiber membranes, the TVB-N value of turbot fillets increased slowly, and the growth rate was slower than that of other electrospun nanofibers ( Figure 8 a). 2-TBA is an important indicator used to describe the degree of fat oxidation in aquatic products. Unsaturated fatty acids contained in aquatic products react with oxygen to produce a series of substances with unpleasant odors such as aldehydes, ketones, and fatty acids, causing rancidity. Therefore, the TBA value can be used to characterize the freshness of aquatic products. Figure 8It can be seen from (b) that the degree of fat oxidation of turbot fillets wrapped with polylactic acid / citral electrospinning nanofiber membrane is significantly lower than that of the control group, and its delaying effect on fat oxidation of turbot fillets is better than other electrospinning. This may be because the polylactic acid / citral electrospinning nanofiber membrane can wrap citral well and can achieve a sustained release effect. The slowly released citral acts as a quorum sensing inhibitor to inhibit the corruption characteristics of aquatic product spoilage bacteria, while other groups of electrospinning fibers have beads and other defects, and the sustained release effect is poor, so the preservation effect on aquatic products is poor. The above results show that the polylactic acid / citral electrospinning nanofiber membrane of the present invention can well maintain the quality and freshness of turbot fillets under refrigerated conditions.

[0083] In summary, the polylactic acid / citral electrospun nanofiber membrane prepared by the present invention has a smooth surface and high mechanical strength. The natural product citral is wrapped with a green and degradable polylactic acid material. It has a wide source, low price, good safety and high efficiency, and can not only block the quorum sensing system of Pseudomonas fluorescens and inhibit its corruption characteristics, but also will not cause bacteria to develop drug resistance. The citral slowly released by the polylactic acid / citral electrospun nanofiber membrane during the refrigeration process can inhibit the increase of volatile basic nitrogen and fat oxidation value related to corruption of turbot fillets during the refrigeration process, delay the corruption and deterioration of aquatic products, have a good maintenance effect on the preservation of aquatic products such as turbot, and have extremely strong application value in the field of aquatic product preservation.

[0084] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.

Claims

1. A polylactic acid / citral electrospinning nanofiber membrane, characterized in that: The preparation method is as follows: Add polylactic acid to a mixed solution of dichloromethane and DMF in a volume ratio of 1:1, stir and dissolve to obtain a polylactic acid solution with a mass fraction of 10%. The solution is magnetically stirred for 12 hours and ultrasonically treated for 2 hours to obtain a polylactic acid shell spinning solution. Citral is prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution. The polylactic acid shell spinning solution and the core spinning solution are placed in syringes respectively. Electrospinning equipment: polylactic acid flow rate: 0.005mm / min, citral flow rate: 0.2mm / min; positive voltage is 24.58kV, negative voltage is 1.64kV, and tin foil is used for receiving. The receiving distance is 20cm and the receiving time is 2h to obtain a polylactic acid / citral electrospinning nanofiber membrane.

2. The method for preparing the polylactic acid / citral electrospinning nanofiber membrane according to claim 1, characterized in that: Here are the steps: Add polylactic acid to a mixed solution of dichloromethane and DMF in a volume ratio of 1:1, stir and dissolve to obtain a polylactic acid solution with a mass fraction of 10%. The solution is magnetically stirred for 12 hours and ultrasonically treated for 2 hours to obtain a polylactic acid shell spinning solution. Citral is prepared into a solution with a volume fraction of 1% with 70% methanol as the core spinning solution. The polylactic acid shell spinning solution and the core spinning solution are placed in syringes respectively. Electrospinning equipment: polylactic acid flow rate: 0.005mm / min, citral flow rate: 0.2mm / min; positive voltage is 24.58kV, negative voltage is 1.64kV, and tin foil is used for receiving. The receiving distance is 20cm and the receiving time is 2h to obtain a polylactic acid / citral electrospinning nanofiber membrane.

3. Application of the polylactic acid / citral electrospun nanofiber membrane prepared according to the method of claim 2 in food preservation.

4. The use according to claim 3, characterized in that: The food is aquatic product.

5. A method for preserving turbot fish meat, characterized in that: The polylactic acid / citral electrospun nanofiber membrane prepared by the method of claim 2 is peeled off from the tin foil, vacuum dried, and then irradiated under ultraviolet light for 15 minutes, used to wrap turbot meat, and stored at 0°C.

6. Use of the polylactic acid / citral electrospun nanofiber membrane prepared according to the method of claim 2 in preparing food packaging materials with antiseptic and fresh-keeping effects.

7. The use according to claim 6, characterized in that: The food is aquatic product.

8. A food packaging material with antiseptic and fresh-keeping effects, characterized in that: A polylactic acid / citral electrospun nanofiber membrane prepared by the method of claim 2.

Citation Information

Patent Citations

  • Methods for treating lignocellulosic materials

    CN104411712A

  • Beaded electrospun nanofiber immobilized saccharomycete and preparation method thereof

    CN105802950A

  • Preparation method of easily-degradable food preservative film with fish scale gelatin matrix

    CN111349343A

  • Antibacterial and disinfectant nanofiber medical dressing and preparation method

    CN113846419A

  • pH sensitive nanofiber web using eletrospinning and process for preparing the same

    KR1020110018114A