A non-alloy steel wire rod for communication cables and its preparation method and application
By adding B, La and Ce elements to non-alloy steel strips and adopting specific smelting and rolling processes, the problem of poor conductivity is solved, the conductivity and plasticity is improved, and its high-end cable field is promoted. Application.
Patent Information
- Application Number
- CN202310238640.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-10
AI Technical Summary
The poor conductivity of existing non-alloy steel strips limits their promotion and application in the fields of copper-clad steel wire composite materials and cables.
By adding B, La and Ce elements to the components of non-alloy steel strips and controlling their reasonable addition amount, the structural structure of the steel is changed, and the precipitation of three cementites at the ferrite grain boundaries are reduced, and specific smelting is adopted Process and rolling processes, including water-desulfurization pretreatment, converter smelting, vacuum refining, casting, controlled rolling and cold rolling and silk spinning processes, controlling ferrite grain size and inclusion composition.
It effectively improves the conductivity of non-alloy steel coils, reduces the degree of work hardening and production costs, and promotes its application in the fields of communication cables, automotive cables, power cables and special cables.
Smart Images

Figure CN116426817B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of production of non-alloy steel wires for communication cables, and in particular to a non-alloy steel wire rod for communication cables, and a preparation method and application thereof. Background Art
[0002] High-end cables used in high-tech fields such as aerospace, automobiles, electronics, and new energy are an important type of precision conductor. They are characterized by single or twisted wires made of thin, ultra-long, high-performance copper alloys or copper-based composite materials through electroplating, and are wrapped with polymer insulation layers and metal shielding layers on the outer layer. They are required to have high conductivity, high strength, good plasticity, high temperature resistance, and strong oxidation resistance. It is an indispensable basic material widely used in high-tech fields, and is responsible for current transmission and signal transmission under special environments.
[0003] However, the electrical conductivity of current non-alloy steel wire rods is generally poor, which, to a certain extent, restricts the promotion and application of non-alloy steel wire rods in the field of copper-clad steel wire composite metal materials and cables. Summary of the invention
[0004] The present application provides a non-alloy steel wire rod for communication cables and a preparation method and application thereof, so as to improve the problem of poor electrical conductivity of the current non-alloy steel wire rod.
[0005] In a first aspect, the present application provides a non-alloy steel wire rod for communication cables, wherein the composition of the non-alloy steel wire rod comprises, by mass fraction: C: 0.001% to 0.025%, Mn: 0.005% to 0.10%, Si: ≤0.03%, P: ≤0.010%, S: ≤0.008%, Al t : ≤0.010%, B: 0.0010%~0.0060%, La: 0.0005%~0.0050%, Ce: 0.0005%~0.0050%, O: ≤0.010%, N: ≤0.004%, the rest are Fe and unavoidable impurities.
[0006] As an optional embodiment, the composition of the non-alloy steel wire rod includes, by mass fraction: C: 0.010% to 0.020%, Mn: 0.03% to 0.07%, Si: ≤0.03%, P: ≤0.010%, S: ≤0.008%, Al t : ≤0.010%, B: 0.0030%~0.0040%, La: 0.0015%~0.0040%, Ce: 0.0015%~0.0040%, O: ≤0.010%, N: ≤0.004%, the rest are Fe and unavoidable impurities.
[0007] As an optional implementation, in the composition of the non-alloy steel wire rod, the relationship between the mass fraction of Al [Al] and the mass fraction of O [O] satisfies: [Al] / [O]=0.7-1.3.
[0008] In a second aspect, the present application provides a method for preparing a non-alloy steel wire rod for a communication cable, wherein the non-alloy steel wire rod is the non-alloy steel wire rod described in the first aspect; the method comprises:
[0009] Obtaining a casting billet;
[0010] The cast billet is heated, and then controlled rolling and controlled cold rolling is performed to obtain a rolled intermediate billet;
[0011] The rolling intermediate billet is subjected to sizing rolling and then wire drawing to obtain non-alloy steel wire rod.
[0012] As an optional implementation manner, the start rolling temperature of the controlled rolling and controlled cold rolling is 980-1100° C.; and / or
[0013] The finishing temperature of the controlled rolling and controlled cold rolling is above 945°C.
[0014] As an optional implementation manner, the finishing temperature of the controlled rolling and controlled cold rolling is 945-980°C.
[0015] As an optional embodiment, the spinning temperature is 880-980° C.; or
[0016] The spinning temperature is 945-980°C; and / or
[0017] The wire drawing includes rough drawing deformation and wet drawing deformation. The rough drawing deformation passes are 7 to 9 passes, the total area reduction rate of the rough drawing deformation is 80 to 95%, and the area reduction rate of each rough drawing pass is 28 to 38%; the wet drawing deformation passes are 8 to 10 passes, the total area reduction rate of the wet drawing deformation is 60 to 80%, and the area reduction rate of each wet drawing pass is 18 to 28%.
[0018] As an optional embodiment, the heating temperature is 1000-1200° C.; and / or
[0019] The heating time is ≥2h.
[0020] As an optional embodiment, the cooling adopts 13-section roller cooling, and the speed of each roller in the 13-section roller cooling is: 0.18m / s-0.20m / s-0.21m / s-0.22m / s-0.23m / s-0.24m / s-0.26m / s-0.30m / s-0.30m / s-0.30m / s-0.40m / s-0.40m / s-0.40m / s-0.40m / s.
[0021] As an optional embodiment, the obtaining of the ingot comprises: pre-treating molten iron for desulfurization to obtain desulfurized molten iron; smelting the desulfurized molten iron in a converter to obtain molten steel in a converter; refining the molten steel in a converter to obtain refined molten steel; casting the refined molten steel to obtain the ingot; and / or
[0022] The desulfurization pretreatment adopts KR stirring deep desulfurization treatment, and the mass content of sulfur in the desulfurized iron water is ≤0.0010%; and / or
[0023] The converter smelting includes electric furnace smelting or top and bottom combined blowing converter smelting, the converter smelting adopts double slag method deep dephosphorization control, and the slag basicity R is controlled to be 3.5-5.0; after the converter smelting is completed, the top slag is modified, the top slag of the top slag modification treatment includes high calcium aluminum slag balls, and the mass content of aluminum in the high calcium aluminum slag balls is ≥50%; and / or
[0024] The refining includes LF refining, VD vacuum refining or RH vacuum refining, wherein the LF refining adopts a light treatment mode, the VD vacuum refining or RH vacuum refining adopts a narrow range oxygen activity control process, the oxygen activity of the narrow range oxygen activity control process is 10-30ppm, the VD vacuum refining or RH vacuum refining adopts a low aluminum-oxygen ratio control technology, the mass content of Al [Al] in the steel of the low aluminum-oxygen ratio control technology is controlled to be ≤0.01%, the mass content of O [O] is controlled to be ≤0.01%, and [Al] / [O] is controlled to be 0.7-1.3; the VD vacuum refining or RH vacuum refining adopts batch addition of ferroborium alloy; the VD vacuum refining or RH vacuum refining adopts low vacuum control to complete deep denitrification, and the mass content of N in the steel after deep denitrification is ≤0.004%;
[0025] The casting adopts a square billet full protection machine casting, and the crystallizer feeding rare earth wire processing technology is adopted during the casting.
[0026] In a third aspect, the present application provides an application of a non-alloy steel wire rod, the application comprising using the non-alloy steel wire rod for communication cables, automotive cables, power cables and special cables, the non-alloy steel wire rod being the non-alloy steel wire rod described in the first aspect.
[0027] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0028] The non-alloy steel wire rod for communication cables provided in the embodiment of the present application can effectively change the organizational structure of the non-alloy steel by adding elements such as B, La and Ce to the composition and controlling their reasonable addition amounts. The ferrite grain size can be controlled to 5.0-6.0 level, reducing the amount of tertiary cementite precipitation at the ferrite grain boundary, and effectively improving the conductivity of the non-alloy steel wire rod, which can reach 16-19%. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0030] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0031] Figure 1 A flowchart of a method provided in an embodiment of the present application. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0034] At present, wire-making enterprises mainly use ultra-low carbon steel wire rods to draw and process copper-clad steel wire bimetallic composite materials. Relevant research has been carried out on the control and detection methods of the conductivity index of ultra-low carbon steel wire rods for wire making. Among them, the key influencing factors of the conductivity index have not been elaborated and explained in detail, and the fluctuation range of the influencing factors corresponding to the fluctuation range of the conductivity index has not given specific parameter values. For the preparation of copper-clad steel wire bimetallic composite materials, copper-clad steel wire is processed and manufactured by electroplating, coating and hot dip continuous casting. Among them, the electroplating method pre-plates and copper-plates the steel wire in an alkaline electrolyte containing cyanide. The disadvantage of this method is that the plating solution contains cyanide components, which are toxic, pollute the environment, and are harmful to the health of workers. In addition, the process is complicated and the production cost is high. A scheme has been proposed to use reels of different diameters for drawing to obtain filaments of required specifications. This method does not perform intermediate heat treatment, and cannot avoid excessive hardening of the finished wire. It cannot be used for products requiring low tensile strength. Another proposal proposes a method for measuring the conductivity of copper-clad steel wire, which mainly solves the influence of different measurement temperatures on the conductivity of the wire, and provides a correction coefficient to correct the measurement results at different temperatures. However, there are many factors that affect the accuracy of the conductivity measurement of metal materials, among which the measurement temperature, the preparation accuracy of the test sample and other factors have a great influence on the measured value of the conductivity. If the correction coefficient is used for correction, the error will be greater.
[0035] In summary, the above methods have not solved the problems related to the control of conductivity index and large error of detection results of ultra-low carbon steel wire rod for copper-clad steel wire, which to a certain extent further restricts the promotion and application of non-alloy steel wire rod in the field of copper-clad steel wire composite metal materials and cables.
[0036] Non-alloy steel wire rod has certain special uses. By effectively controlling the range of key elements in steel, establishing a corresponding relationship between carbon equivalent and key elements in steel, accurately controlling the size and content of inclusions in steel, accurately controlling the total content of residual elements in steel, and appropriately adding rare earth elements and boron elements, the composition and organizational structure of inclusions in steel are changed, the plasticity index and electrical conductivity of non-alloy steel wire rod are improved, effectively promoting the promotion and application of non-alloy steel wire rod in the fields of communication cables, automotive cables, power cables and special cables.
[0037] The present application provides a high-plasticity non-alloy steel wire rod for communication cables and its production and preparation method and application. Through the design of key components of non-alloy steel wire rods, the setting and control of key smelting processes and rolling process parameters, and the research and development and application of rare earth element modification technology, high-plasticity non-alloy steel wire rods for communication cables can be manufactured. The problem of high strength, poor plasticity during drawing and low conductivity index of low-carbon steel and ultra-low-carbon steel wire rods prepared by the prior art is solved.
[0038] like Figure 1 As shown, the embodiment of the present application provides a non-alloy steel wire rod for communication cables, wherein the composition of the non-alloy steel wire rod includes, by mass fraction: C: 0.001% to 0.025%, Mn: 0.005% to 0.10%, Si: ≤0.03%, P: ≤0.010%, S: ≤0.008%, Al t : ≤0.010%, B: 0.0010%~0.0060%, La: 0.0005%~0.0050%, Ce: 0.0005%~0.0050%, O: ≤0.010%, N: ≤0.004%, the rest are Fe and unavoidable impurities.
[0039] The main function of C is to change the mechanical properties of non-alloy steel wire rod. The reason for controlling the mass fraction of C to 0.001%~0.025% is that the tensile strength of the non-alloy steel wire rod can be controlled within a certain range. The adverse effect of too large a mass fraction is that the strength of the non-alloy steel wire rod is too high, resulting in poor plasticity. The adverse effect of too small a mass fraction is that the elastic index of the non-alloy steel wire rod does not meet the requirements.
[0040] The main function of Mn is to change the electrical conductivity of non-alloy steel wire rod. The reason for controlling the mass fraction of Mn to 0.005% to 0.10% is that the electrical conductivity of non-alloy steel wire rod can be controlled within a certain range. If the mass fraction is too large, the adverse effect is that the electrical conductivity of non-alloy steel wire rod is too low, and if the mass fraction is too small, the adverse effect is that the electrical conductivity of non-alloy steel wire rod is too high, which is not conducive to the processing and manufacturing of blasting lead materials.
[0041] The main function of Si is to change the inclusion composition of non-alloy steel wire rod. The reason for controlling the mass fraction of Si to ≤0.03% is to reduce the number of Class C inclusions generated in non-alloy steel wire rod. The adverse effect of taking too large a mass fraction is that the Class C inclusions in non-alloy steel wire rod exceed the standard.
[0042] The main function of Al is to change the cleanliness of non-alloy steel wire rod and control the castability during billet production. The reason for controlling the mass fraction of Al to ≤0.010% is to ensure the castability continuity and cleanliness of non-alloy steel billets. The adverse effect of taking an excessively large mass fraction is that it causes the alloy steel billet to be easily blocked in the water nozzle during continuous casting production, affecting the castability control of continuous casting.
[0043] The main function of B is to change the organizational structure of non-alloy steel wire rod. The reason for controlling the mass fraction of B to 0.0010%~0.0060% is that it can stably control the ferrite grain size and mechanical properties of non-alloy steel wire rod. The adverse effect of too large a mass fraction is that the ferrite grain size of the non-alloy steel wire rod is too small, the ferrite grain size is too large, and the mixed crystal problem is easy to occur, and the uniformity of the mechanical properties of the wire rod becomes worse. The adverse effect of too small a mass fraction is that the ferrite grain size of the non-alloy steel wire rod is too large, the ferrite grain size is too small, and the yield strength of the non-alloy steel wire rod is too low.
[0044] The main function of Ce is to change the inclusion composition of non-alloy steel. The reason for controlling the mass fraction of Ce to 0.0005% to 0.0050% is that it can effectively change the inclusion structure of non-alloy steel. The adverse effect of too large a mass fraction is that it will cause cracks in the non-alloy steel ingot, and the adverse effect of too small a mass fraction is that it cannot achieve the effect of changing the inclusion structure of non-alloy steel.
[0045] The main function of O is to affect the cleanliness of non-alloy steel and the surface quality of continuous casting billets. The reason for controlling the mass fraction of O ≤ 0.010% is to ensure the continuous casting castability of non-alloy steel billets. The adverse effect of taking an excessively large mass fraction is that it will cause pores on the surface of the non-alloy steel billet and affect the surface quality of the non-alloy steel wire rod.
[0046] The main function of N is to affect the mechanical properties and drawing effect of non-alloy steel wire rod. The reason for controlling the mass fraction of N to ≤0.004% is that it can stably control the tensile strength of non-alloy steel wire rod. The adverse effect of taking a too large mass fraction is that the strength of non-alloy steel wire rod is too high and the wire is prone to breakage during the wire rod drawing process.
[0047] In some embodiments, the composition of the non-alloy steel wire rod includes, by mass fraction: C: 0.010% to 0.020%, Mn: 0.03% to 0.07%, Si: ≤0.03%, P: ≤0.010%, S: ≤0.008%, Al t : ≤0.010%, B: 0.0030%~0.0040%, La: 0.0015%~0.0040%, Ce: 0.0015%~0.0040%, O: ≤0.010%, N: ≤0.004%, the rest are Fe and unavoidable impurities.
[0048] In some embodiments, in the composition of the non-alloy steel wire rod, the relationship between the mass fraction of Al [Al] and the mass fraction of O [O] satisfies: [Al] / [O]=0.7-1.3.
[0049] By controlling the low aluminum and low oxygen content in the steel, [Al]≤0.005%, [O]≤0.005%, [Al] / [O]=0.7~1.3, low-content small-size inclusions can be obtained, and the proportion of inclusions ≤5μm can reach more than 90%, which can effectively improve the processing plasticity of non-alloy steel wire rods
[0050] like Figure 1 As shown, based on a general inventive concept, the embodiment of the present application also provides a method for preparing non-alloy steel wire rod for communication cables, wherein the non-alloy steel wire rod is the non-alloy steel wire rod provided above; process technology scheme: hot metal desulfurization pretreatment - electric furnace smelting or top and bottom combined blowing converter smelting - LF refining furnace or VD vacuum refining furnace or RH vacuum refining furnace treatment - square billet full protection casting machine pouring - heating furnace heating - high-speed wire rolling mill controlled rolling and controlled cold rolling - sizing unit rolling - high-speed laying head control - cooling section air cooling and insulation cover control - coiling packaging. The specific method includes:
[0051] S1. Obtaining a cast billet;
[0052] Specifically, in this embodiment, obtaining the ingot specifically includes: molten iron desulfurization pretreatment, electric furnace smelting or top and bottom combined blowing converter smelting, LF refining furnace or VD vacuum refining furnace or RH vacuum refining furnace treatment and square billet full protection casting machine pouring to obtain the ingot.
[0053] Furthermore, KR stirring deep desulfurization treatment is adopted for molten iron pretreatment, and the sulfur content of molten iron after KR treatment reaches the target of ≤0.0010%.
[0054] In the process of electric furnace smelting or top-bottom combined blowing converter smelting, double slag method is adopted for deep dephosphorization control, and the slag basicity R is controlled at 3.5-5.0 to form a composite solid phosphorus phase of calcium phosphate, silicon dioxide and magnesium oxide. After electric furnace smelting or top-bottom combined blowing converter smelting, the ladle top slag modification treatment technology is adopted, and high calcium aluminum slag balls with aluminum content ≥50% are added to the top slag.
[0055] The LF refining furnace adopts a light treatment mode to quickly heat up and homogenize the molten steel; or, when treated in a VD vacuum refining furnace or an RH vacuum refining furnace, a narrow range oxygen activity control process is adopted, the oxygen activity is controlled at 10-30ppm, and a low aluminum-oxygen ratio control technology is adopted, [Al] in the steel is controlled to ≤0.01, [O] in the steel is controlled to ≤0.01, and [Al] / [O] is controlled in the range of 0.7-1.3; boron iron alloy is added in batches, the range of boron element is controlled at 0.0010-0.0060%, low vacuum control is adopted, deep denitrification treatment is carried out, and nitrogen in the steel is controlled to ≤0.004%.
[0056] During the protective casting of square billets, the crystallizer feeding rare earth wire treatment technology is adopted to control the rare earth elements La: 0.0005~0.0050%, Ce: 0.0005~0.0050% in the steel, and the crystallizer electromagnetic stirring + billet end electromagnetic stirring + single roller light pressure control technology are adopted, and special crystallizer protection slag + special high-alkalinity middle bag covering agent + carbon-free ladle are used.
[0057] S2. The ingot is heated, and then subjected to controlled rolling and controlled cold rolling to obtain a rolled intermediate billet;
[0058] In some embodiments, the start rolling temperature of the controlled rolling and controlled cold rolling is 980-1100° C., and the finishing temperature of the controlled rolling and controlled cold rolling is above 945° C. Preferably, the finishing temperature of the controlled rolling and controlled cold rolling is 945-980° C.
[0059] In some embodiments, the heating temperature is 1000-1200° C.; the heating time is ≥2 h.
[0060] S3. The rolled intermediate billet is subjected to sizing rolling and then wire drawing to obtain non-alloy steel wire rod.
[0061] In some embodiments, the spinning temperature is 880-980°C; preferably, the spinning temperature is 945-980°C.
[0062] In this embodiment, the spinning includes rough drawing deformation and wet drawing deformation. The rough drawing deformation is 7 to 9 times, and the total surface reduction rate of the rough drawing deformation is 80 to 95%; the wet drawing deformation is 8 to 10 times, and the total surface reduction rate of the wet drawing deformation is 60 to 80%. In the rough drawing deformation, the surface reduction rate of each drawing is 28 to 38%, and in the wet drawing deformation, the surface reduction rate of each drawing is 18 to 28%; after the spinning is completed, the cooling section is air-cooled and the insulation cover is controlled, and the roller speed of the cooling section is reasonably adjusted. By controlling the roller speed of each section, the circle spacing and cooling speed are controlled. Specifically, 13 sections of rollers are used, and the roller speed of each section (unit: m / s) is: 0.18-0.20-0.21-0.22-0.23-0.24-0.26-0.30-0.30-0.30-0.40-0.40-0.40. An ultra-low roller speed of 0.18m / s and a slow cooling control process with a heat preservation cover are adopted. The fan is closed in sections and the heat preservation cover is opened in sections to ensure stable control of the wire rod cooling rate. The non-alloy steel wire rod is coiled and subjected to incomplete crystallization annealing treatment at 670-720℃ with a heat preservation time of 350-600min to obtain a uniform non-alloy steel wire rod structure.
[0063] The obtained non-alloy steel wire rod has a ferrite grain size grade of 5.0-7.0; the yield strength ratio is controlled at 0.56-0.7; and the diameter of the drawn filament is ≤1.0mm.
[0064] By adopting the above method, controlling the appropriate range of carbon content in steel and controlling the cooling process, low-strength and high-plasticity non-alloy steel wire rod can be obtained. The wire rod yield ratio is controlled to the range of 0.56-0.7, corresponding to a tensile strength of 250-320MPa, an elongation of 35-60%, and a cross-sectional shrinkage rate ≥85%.
[0065] Based on a general inventive concept, an embodiment of the present application also provides an application of a non-alloy steel wire rod, the application comprising using the non-alloy steel wire rod for communication cables, automotive cables, power cables and special cables, and the non-alloy steel wire rod is the non-alloy steel wire rod provided above.
[0066] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0067] Examples 1-4
[0068] A method for preparing non-alloy steel wire rod, the method comprising: hot metal desulfurization and slag removal → 210-ton top and bottom combined blowing converter smelting → slag blocking and steel tapping → ladle deoxidation and alloying → RH vacuum refining → Si-Ca wire feeding → ladle bottom blowing argon soft blowing → 130mm 2 Continuous casting machine with full protection casting → Billet surface inspection → High-speed wire mill rolling mill to produce ¢6.5~14mm wire rod → Wire rod inspection → Finished product packaging and storage.
[0069] 1) The molten iron is pretreated for desulfurization to ensure that the sulfur content of the molten iron entering the converter reaches 0.005%;
[0070] 2) Top and bottom combined blowing converter smelting, slag blocking steel tapping, steel tapping temperature 1710℃;
[0071] 3) Use medium carbon ferromanganese for final deoxidation, with an addition amount of 1.0-3.5 kg / t steel, and calculate the amount of converter deoxidation alloy added based on the converter endpoint composition;
[0072] 4) RH refining lifting ladle, evacuate the vacuum to make the vacuum degree ≤50mbar; decarburize the molten steel by vacuum decarburization or light treatment to make the target C ≤0.01%; after the RH vacuum decarburization is completed, the oxygen is determined, and the molten steel is deoxidized with aluminum particles, low-carbon ferromanganese, and carbon powder, and the target oxygen activity is controlled at 15ppm;
[0073] 5) The small square billet casting machine adopts full protection casting method, the tundish is equipped with a slag retaining wall, and the liquid level in the tundish is > 600mm; the crystallizer adopts electromagnetic stirring, and the tundish uses a low-carbon and high-basicity covering agent;
[0074] 6) Heating temperature: 1100℃, rolling temperature: 1040℃, spinning temperature: 920℃.
[0075] 7) Speed of each roller in cooling section (unit: m / s):
[0076] 0.18-0.20-0.21-0.22-0.23-0.24-0.26-0.30-0.30-0.30-0.40-0.40-0.40.
[0077] All fans are turned off and all heat preservation covers are opened to make the wire rod cool evenly. The ferrite grain size of ultra-low carbon steel wire rod is controlled at 20-40μm, the tertiary cementite content is ≤2%, the tensile strength is ≤290MPa, the surface shrinkage is ≥85%, and the performance difference of the same circle is ≤20Mpa.
[0078] The chemical composition (wt%) of each embodiment is shown in the following table:
[0079] C(%) Si(%) Mn(%) P(%) S(%) B(%) Example 1 0.005 0.010 0.05 0.004 0.002 0.0022 Example 2 0.007 0.012 0.03 0.006 0.004 0.0025 Example 3 0.003 0.015 0.04 0.0035 0.005 0.0015 Example 4 0.002 0.02 0.08 0.009 0.003 0.0035
[0080] The performance of the 10 ¢6.5 mm non-alloy steel wire rods provided in Examples 1-4 was tested, and the results are shown in the following table:
[0081]
[0082]
[0083] Embodiment 5-8
[0084] A method for preparing non-alloy steel wire rod, the method comprising: hot metal desulfurization and slag removal → 100-ton electric furnace smelting → slag blocking and steel tapping → ladle deoxidation and alloying → LF refining → VD vacuum refining → Si-Ca wire feeding → ladle bottom blowing argon soft blowing → 160mm 2 Continuous casting machine with full protection casting → Billet surface inspection → High-speed wire mill rolling mill to produce ¢6.5~20mm wire rod → Wire rod inspection → Finished product packaging and storage.
[0085] 1) The molten iron is pretreated for desulfurization to ensure that the sulfur content of the molten iron entering the converter reaches 0.005%;
[0086] 2) Using electric furnace smelting, slag blocking steel tapping, steel tapping temperature 1663℃;
[0087] 3) Use low carbon ferromanganese for final deoxidation, adding 2.0kg / t steel, and calculate the amount of converter deoxidation alloy added according to the converter endpoint composition;
[0088] 4) VD refining lifting ladle, evacuation, so that the vacuum degree ≤ 60mbar; make the target C ≤ 0.01%; after the VD vacuum decarburization is completed, the oxygen is determined, and the molten steel is deoxidized with aluminum particles, low-carbon ferromanganese, and carbon powder, and the target oxygen activity is controlled at 18ppm;
[0089] 5) The small square billet casting machine adopts full protection casting method, the tundish is equipped with a slag retaining wall, and the liquid level in the tundish is > 600mm; the crystallizer adopts electromagnetic stirring, and the tundish uses a low-carbon and high-basicity covering agent;
[0090] 6) Heating temperature: 1150℃, rolling temperature: 990℃, spinning temperature: 930℃.
[0091] 7) Speed of each roller in cooling section (unit: m / s):
[0092] 0.18-0.20-0.21-0.22-0.23-0.24-0.26-0.30-0.30-0.30-0.40-0.40-0.40.
[0093] All fans are turned off and all heat preservation covers are opened to make the wire rod cool evenly. The ferrite grain size of ultra-low carbon steel wire rod is controlled at 20-40μm, the tertiary cementite content is ≤2%, the tensile strength is ≤290MPa, the surface shrinkage is ≥85%, and the performance difference of the same circle is ≤20Mpa.
[0094] The chemical composition (wt%) of each embodiment is shown in the following table:
[0095] C(%) Si(%) Mn(%) P(%) S(%) B(%) Example 5 0.008 0.015 0.045 0.0035 0.006 0.0032 Example 6 0.012 0.018 0.058 0.007 0.008 0.0038 Example 7 0.009 0.020 0.038 0.005 0.005 0.0026 Example 8 0.014 0.024 0.09 0.008 0.007 0.0047
[0096] The performance of the 10 ¢7.5 mm non-alloy steel wire rods provided in Examples 5-8 was tested, and the results are shown in the following table:
[0097]
[0098]
[0099] Examples 9-12
[0100] A method for preparing non-alloy steel wire rod, comprising: hot metal desulfurization and slag removal → 150-ton top and bottom combined blowing converter smelting → slag blocking and steel tapping → ladle deoxidation and alloying → RH vacuum refining → Si-Ca wire feeding → ladle bottom blowing argon soft blowing → 200mm 2 Continuous casting machine with full protection casting → Billet surface inspection → High-speed wire mill rolling mill to produce ¢6.5~30mm wire rod → Wire rod inspection → Finished product packaging and storage.
[0101] 1) The molten iron is pretreated for desulfurization to ensure that the sulfur content of the molten iron entering the converter reaches 0.005%;
[0102] 2) Top and bottom combined blowing converter smelting, slag blocking steel tapping, steel tapping temperature 1685℃;
[0103] 3) Use low carbon ferromanganese for final deoxidation, the addition amount is 2.15kg / t steel, and the addition amount of converter deoxidation alloy is calculated according to the converter end point composition;
[0104] 4) RH refining lifting ladle, evacuating the vacuum to make the vacuum degree ≤30mbar; decarburizing the molten steel by vacuum decarburization to make the target C ≤0.005%; after the RH vacuum decarburization, the oxygen is determined, and the molten steel is deoxidized with aluminum particles, low-carbon ferromanganese, and carbon powder, and the target oxygen activity is controlled at 10-20ppm;
[0105] 5) The small square billet casting machine adopts full protection casting method, the tundish is equipped with a slag retaining wall, and the liquid level in the tundish is > 600mm; the crystallizer adopts electromagnetic stirring, and the tundish uses a low-carbon and high-basicity covering agent;
[0106] 6) Heating temperature: 1200℃, rolling temperature: 1060℃, spinning temperature: 900℃.
[0107] 7) Speed of each roller in cooling section (unit: m / s):
[0108] 0.18-0.20-0.21-0.22-0.23-0.24-0.26-0.30-0.30-0.30-0.40-0.40-0.40.
[0109] All fans are turned off and all heat preservation covers are opened to make the wire rod cool evenly. The ferrite grain size of ultra-low carbon steel wire rod is controlled at 20-40μm, the tertiary cementite content is ≤2%, the tensile strength is ≤290MPa, the surface shrinkage is ≥85%, and the performance difference of the same circle is ≤20Mpa.
[0110] The chemical composition (wt%) of each embodiment is shown in the following table:
[0111] C(%) Si(%) Mn(%) P(%) S(%) B(%) Example 9 0.0010 0.008 0.020 0.003 0.0025 0.0015 Example 10 0.0012 0.010 0.030 0.005 0.003 0.0020 Embodiment 11 0.0015 0.006 0.025 0.0035 0.004 0.0025 Example 12 0.0016 0.005 0.030 0.007 0.0028 0.0045
[0112] The performance of the 10 ¢8 mm non-alloy steel wire rods provided in Examples 9-12 was tested, and the results are shown in the following table:
[0113]
[0114]
[0115] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0116] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present specification, the terms "including", "comprising", etc. refer to "including but not limited to". In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of the associated objects, indicating that there may be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A, B can be singular or plural. In this article, "at least one" refers to one or more, and "plural" refers to two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of singular or plural items. For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0117] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A non-alloy steel wire rod for communication cables, characterized in that: The composition of the non-alloy steel wire rod is calculated by mass fraction as follows: C: 0.010% to 0.020%, Mn: 0.03% to 0.07%, Si: ≤0.03%, P: ≤0.010%, S: ≤0.008%, Al: ≤0.010%, B: 0.0030% to 0.0040%, La: 0.0015% to 0.0040%, Ce: 0.0015% to 0.0040%, O: ≤0.010%, N: ≤0.004%, and the rest is Fe and unavoidable impurities; The preparation method of the non-alloy steel wire rod comprises: Performing desulfurization pretreatment on molten iron to obtain desulfurized molten iron; Performing converter smelting on the desulfurized molten iron to obtain converter molten steel; Refining the converter molten steel to obtain refined molten steel; Casting the refined molten steel to obtain a casting billet; The cast billet is heated, and then controlled rolling and controlled cold rolling is performed to obtain a rolled intermediate billet; The rolling intermediate billet is subjected to sizing rolling, followed by wire drawing and cooling treatment to obtain a non-alloy steel wire rod; The refining includes LF refining, VD vacuum refining or RH vacuum refining, wherein the LF refining adopts a light treatment mode, the VD vacuum refining or RH vacuum refining adopts a narrow range oxygen activity control process, the oxygen activity of the narrow range oxygen activity control process is 10-30ppm, the VD vacuum refining or RH vacuum refining adopts a low aluminum-oxygen ratio control technology, the mass fraction of Al [Al] in the steel using the low aluminum-oxygen ratio control technology is controlled to be ≤0.01%, the mass fraction of O [O] is controlled to be ≤0.01%, and [Al] / [O] is controlled to be 0.7-1.3; the VD vacuum refining or RH vacuum refining adopts batch addition of ferroboron alloy to control the mass fraction of B in the steel to be 1.111%-1.0060%; the VD vacuum refining or RH vacuum refining adopts low vacuum control to complete deep denitrification, and the mass fraction of N in the steel after deep denitrification is ≤0.004%; The casting adopts a square billet full protection machine casting, and the casting adopts a crystallizer feeding rare earth wire processing technology to control the mass fraction of La and Ce in the steel to meet the following conditions: La: 0.0015%~0.0040%, Ce: 0.0015%~0.0040%, and the casting adopts a crystallizer electromagnetic stirring + billet end electromagnetic stirring + single roller light pressure control technology; The spinning process includes rough drawing deformation and wet drawing deformation, the rough drawing deformation process is 7 to 9 passes, the total area reduction rate of the rough drawing deformation is 80 to 95%, and the area reduction rate of each rough drawing process is 28 to 38%; the wet drawing deformation process is 8 to 10 passes, the total area reduction rate of the wet drawing deformation is 60 to 80%, and the area reduction rate of each wet drawing process is 18 to 28%; The cooling adopts 13-section roller cooling, and the speed of each roller in the 13-section roller cooling is: 0.18 m / s -0.20 m / s -0.21 m / s -0.22 m / s -0.23 m / s -0.24 m / s-0.26 m / s -0.30 m / s -0.30 m / s -0.30 m / s-0.40 m / s -0.40 m / s -0.40 m / s; The non-alloy steel wire rod has a ferrite grain size of 5.0 to 7.0; a yield ratio of 0.56 to 0.7; a diameter of the drawn filament of ≤1.0 mm, an elongation of 35-60%, a cross-sectional shrinkage of ≥85%, and a conductivity of 16-19%.
2. The non-alloy steel wire rod for communication cables according to claim 1, characterized in that: In the composition of the non-alloy steel wire rod, the relationship between the mass fraction of Al [Al] and the mass fraction of O [O] satisfies: [Al] / [O]=0.7~1.
3.
3. The non-alloy steel wire rod for communication cables according to claim 1, characterized in that: The heating temperature is 1000-1200° C.; and / or The heating time is ≥ 2h; and / or The start rolling temperature of the controlled rolling and controlled cold rolling is 980-1100° C.; and / or The finishing temperature of the controlled rolling and controlled cold rolling is above 945°C.
4. The non-alloy steel wire rod for communication cables according to claim 1, characterized in that: The finishing temperature of the controlled rolling and controlled cold rolling is 945-980°C.
5. The non-alloy steel wire rod for communication cables according to claim 4, characterized in that: The spinning temperature is 880-980°C.
6. The non-alloy steel wire rod for communication cables according to claim 1, characterized in that: The desulfurization pretreatment adopts KR stirring deep desulfurization treatment, and the mass fraction of sulfur in the desulfurized iron water is ≤0.0010%; The converter smelting includes electric furnace smelting or top and bottom combined blowing converter smelting, the converter smelting adopts double slag method deep dephosphorization control, and the slag basicity R is controlled to be 3.5-5.0; after the converter smelting is completed, the top slag is modified, and the top slag of the top slag modification treatment includes high calcium aluminum slag balls, and the mass fraction of aluminum in the high calcium aluminum slag balls is ≥50%.
7. The non-alloy steel wire rod for communication cables according to claim 4, characterized in that: The spinning temperature is 945-980°C.
8. An application of non-alloy steel wire rod, characterized in that: The application includes using the non-alloy steel wire rod for communication cables, automotive cables, power cables and special cables, and the non-alloy steel wire rod is the non-alloy steel wire rod according to any one of claims 1 to 7.
Citation Information
Patent Citations
Steel bar or steel claw section for electric conduction of electrolytic aluminum and manufacturing method of steel bar or steel claw section
CN103305747A
Semi-hard type cable steel and production method thereof
CN107236902A
Steel wire rod for copper clad steel composite shielded wire and production method of steel wire rod
CN108062992A
Wire rod for prestressed steel strand and production process of wire rod
CN115261735A
Production of thick steel plate excellent in toughness
JP1997176730A