Flexible MOFs-based boron affinity molecular imprinted membrane adsorbent and preparation method and application thereof
The flexible polymer chain covalently connects MOFs crystals and introduces boric acid monomers to prepare boron affinity molecular imprinted film, solving the problems of poor selectivity and low yield in naringin extraction method, and achieving efficient selective separation of naringin and Enriched, with excellent separation ability and pH response function.
Patent Information
- Application Number
- CN202310642622.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-06-01
AI Technical Summary
The existing naringin extraction methods have poor selectivity, low target product yield and low reuse rate. The selective separation and purification ability of boron affinity adsorbents to naringin are limited, making it difficult to achieve efficient separation and effective utilization of resources.
The crystals of metal organic frame materials (MOFs) are covalently connected by flexible polymer chains, boric acid monomers are introduced, and a MOF-based boron affinity molecular imprinted film with boric acid functionalization is prepared by light-induced synthesis method for selectivity of naringin Separation. The specific steps include copolymerization of the modified H-UiO-66-NH-Met with the acrylate monomer and the boric acid monomer, and then polymerization under the action of a photoinitiator to prepare a flexible MOFs-based boron affinity molecular imprinted film adsorbent.
It realizes efficient selective separation and enrichment of naringin. The material has excellent separation ability, excellent chemical properties and mass transfer kinetic properties, and has pH response function, which simplifies adsorption and desorption operation.
Smart Images

Figure CN116440878B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of environmental functional materials, and relates to a preparation method and application of a flexible MOFs-based boron affinity molecular imprinted membrane adsorbent. Background Art
[0002] Naringin is a natural flavonoid compound and an important nutrient in pomelo peel. It has multiple pharmacological activities, such as antioxidant, anticancer, antimicrobial, cardiovascular and cerebrovascular protection, and microcirculation improvement. It is often discarded as waste in agricultural production, causing environmental pollution and waste of resources. The traditional extraction methods of naringin mainly include acid precipitation and solvent extraction. These methods have their own advantages and disadvantages, but their common defects are poor selectivity, low yield of target products and low reuse rate. Boron affinity adsorbents have become important adsorbents for separation and enrichment of flavonoid compounds. The selectivity of boron affinity for ortho-dihydroxy compounds is based on the fact that the boric acid group can form a reversible five-membered ring ester with the ortho-dihydroxy functional group. The reversible adsorption and release of ortho-dihydroxy compounds can be achieved by pH regulation. As a typical ortho-cis-dihydroxy compound, naringin has a specific affinity for boric acid-based adsorbents, which is expected to achieve its selective separation and purification. Therefore, establishing and improving a new mechanism for the selective identification, separation and purification of naringin, which can efficiently separate pollutants and has acid-base controlled release performance, and improve selectivity while increasing product yield, has important theoretical significance and long-term practical value.
[0003] Currently, metal organic framework (MOF) thin films can be prepared by direct solvothermal synthesis, secondary growth, electrochemical methods, assembly of preformed MOF nanocrystals, liquid phase epitaxy, and Langmuir-Blodgett layer-by-layer deposition to grow MOF layers on certain substrates. The combination of MOFs with polymer matrices endows mixed matrix membranes with the properties of polymers and MOFs. Challenges such as poor compatibility and particle aggregation must be overcome to achieve the desired properties and performance. Despite some progress in recent years, most MOF-based membranes lack uniformity at the molecular level. It is worth noting that supported membranes have been widely used in industrial processes, and this concept can be applied to combine MOF crystals with various substrates to obtain supported MOF membranes. Specifically, some pioneering studies have been conducted on such MOF-based membranes for various applications, including gas separation, chemical sensing, and catalysis. To further understand the basic science and the role of MOF crystals, many MOFs have been chemically modified after synthesis to possess novel and complex properties. There are also other strategies, including cation exchange, linker exchange and post-synthesis metallization, which are also used to adjust the properties of MOFs. The development of various MOFs-based composite materials has attracted the interest of a large number of scientific researchers. Summary of the invention
[0004] The invention discloses a fast and convenient method for covalently linking MOFs crystals in an orderly manner through flexible polymer chains, namely post-synthesis polymerization (PSP), by introducing boric acid monomers as functional monomers. In this way, MOFs with polymerizable functional groups can be copolymerized with organic monomers to obtain elastic boron affinity imprinted membranes, which are finally used to specifically separate and enrich naringin molecules; specifically, the modified H-UiO-66-NH-Met nanoparticles are copolymerized with acrylate monomers and boric acid monomers under ultraviolet light to manufacture an imprinted membrane of a predetermined shape, which is used for the selective separation of naringin. A post-modification molecular imprinting strategy was used to functionalize H-UiO-66-NH-Met with methacrylamide groups. Secondly, the modified H-UiO-66-NH-Met was mixed with butyl methacrylate (BMA) and acrylamidophenylboronic acid under the action of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide. The suspension was then dropped into a polytetrafluoroethylene mold and ultraviolet-initiated polymerization was used to prepare a flexible MOFs-based boron affinity molecular imprinted membrane adsorbent, which was used to selectively separate and enrich NRG molecules.
[0005] The technical solution adopted by the present invention is:
[0006] (1) Preparation of H-UiO-66-NH2
[0007] A certain amount of zirconium chloride, benzoic acid, 2-aminoterephthalic acid and zinc nitrate hexahydrate were added to a certain amount of anhydrous N, N-dimethylformamide solution, ultrasonicated for 30 minutes, and then transferred to a polytetrafluoroethylene reactor at 120°C for continuous reaction for 24 hours. The obtained product was collected by centrifugation and washed with DMF and anhydrous ethanol. The final product was added to a certain amount of hydrochloric acid solution with a pH of 1 and stirred for 15 minutes, then collected by centrifugation and washed with acetone, DMF and anhydrous ethanol in turn, and finally transferred to a vacuum oven and dried overnight at 60°C in vacuum to obtain a mesoporous MOFs material, namely H-UiO-66-NH2.
[0008] In step (1), the zirconium chloride, benzoic acid, 2-aminoterephthalic acid, zinc nitrate hexahydrate, anhydrous N,N-dimethylformamide, and hydrochloric acid solution are added in a ratio of (110-130) mg: (1.82-1.84) g: (180-182) mg: (146-150) mg: (10-30) mL: (10-30) mL.
[0009] (2) Preparation of H-UiO-66-NH-Met
[0010] The H-UiO-66-NH2 prepared in step (1) and methacrylic anhydride BMA are dispersed in a certain amount of chloroform A, and heated at 55-60°C for 24 hours, then centrifuged and washed several times with chloroform, collected and immersed in a certain amount of chloroform B for three days, and the solvent is renewed once a day, and then immersed in methanol for three days, and the solvent is renewed once a day. The centrifuged collection is placed and transferred to a vacuum oven and dried at 150°C for 2 hours to obtain H-UiO-66-NH-Met.
[0011] In step (2), the usage ratio of H-UiO-66-NH2, methacrylic anhydride BMA, chloroform A, chloroform B and methanol is (50-70) mg: (0.15-0.25) mmol: (4-6) mL: (14-16) mL: (14-16) mL.
[0012] (3) Preparation of PBMMA-MOF-MIPs
[0013] A certain amount of H-UiO-66-NH2-Met, acrylamidophenylboronic acid and naringin were suspended in a certain amount of butyl methacrylate (BMA) and ultrasonically treated. A certain amount of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added to the mixture and ultrasonically treated. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under ultraviolet light for 12 to 16 hours. Subsequently, the template was eluted in a certain amount of eluent (methanol: acetic acid volume ratio = 9:1), and the MOF-based boron affinity molecular imprinted membrane PBMMA-MOF-MIPs was obtained after natural air drying.
[0014] The non-imprinted polymer (PBMMA-MOF-NIPs) was prepared by the aforementioned scheme without adding NRG; while the blank flexible independent membrane was prepared without adding H-UiO-66-NH2-Met, acrylamidophenylboronic acid and naringin, and a certain amount of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was directly added to a certain amount of butyl methacrylate (BMA) and ultrasonically treated, and the resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV light for 12 to 16 hours.
[0015] In step (3), the amount ratio of H-UiO-66-NH2-Met, acrylamidophenylboronic acid, naringin, butyl methacrylate (BMA), photoinitiator phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide and eluent is (40-60) mg: (18-19) mg: (7-7.5) mg: (190-210) mg: (15-17) mg: (14-16) mL.
[0016] The flexible porous boron affinity copolymer adsorbent prepared by the invention is used for selective separation of flavonoid compounds.
[0017] The flexible porous boron affinity copolymer adsorbent prepared by the invention is used for the selective separation of ortho-dihydroxy compounds.
[0018] Technical advantages of the present invention:
[0019] The flexible MOFs-based boron affinity molecular imprinted membrane adsorbent prepared by the present invention adopts a quick and simple method of covalently linking MOF crystals in an orderly manner through flexible polymer chains, introduces boric acid monomers as functional monomers, and constructs a molecular imprinted membrane with boric acid functionalized recognition sites through a photoinduced synthesis and post-polymerization method. The material has excellent separation ability, excellent chemical properties and excellent mass transfer kinetics. In addition, the material also has a pH response function to simplify the adsorption and desorption operations. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Scanning images (A, B,) of H-UiO-66-NH2 prepared in Example 1;
[0021] Figure 2 Scanning images of the blank (A1, A2) flexible independent membrane adsorbent and the MOF-based boron affinity molecule non-imprinted (B1, B2) / imprinted (C1, C2) flexible independent membrane adsorbent prepared in Example 1;
[0022] Figure 3 Prepared in Example 1 Figure 3 is the infrared spectrum of PBMMA-MOF-MIPs prepared in Example 1;
[0023] Figure 4 The XPS spectrum of the MOF-based boron affinity molecular imprinted / non-imprinted flexible independent membrane adsorbent prepared in Example 1 and the fine spectrum of B;
[0024] Figure 5 This is an energy spectrum analysis diagram of the MOF-based boron affinity molecular imprinting flexible independent membrane adsorbent prepared in Example 1;
[0025] Figure 6 It is the adsorption kinetics curve of the MOF-based boron affinity molecular imprinted flexible independent membrane adsorbent (PBMMA-MOF-MIPs) in Experimental Example 1;
[0026] Figure 7 The adsorption isotherm curve diagram of the MOF-based boron affinity molecular imprinted flexible independent membrane adsorbent (PBMMA-MOF-MIPs) in Experimental Example 2;
[0027] Figure 8The competitive adsorption bar graph of the MOF-based boron affinity molecular imprinted flexible independent membrane adsorbent (PBMMA-MOF-MIPs) in Experimental Example 3. DETAILED DESCRIPTION
[0028] In the specific implementation of the present invention, the recognition performance evaluation is carried out according to the following method: using a static adsorption experiment. 5 mL of a certain concentration of NRG solution is added to a centrifuge tube, and a certain amount of a three-dimensional flexible boron affinity porous polymer adsorbent is added and placed in a constant temperature water area of 35°C for several hours. After adsorption, the NRG content is measured by a UV-visible spectrophotometer, and the adsorption capacity is calculated based on the results; after saturated adsorption, the three-dimensional flexible boron affinity porous polymer adsorbent is collected by pinching with tweezers, and several hydroxyl compounds with similar structures and properties are selected as competitive adsorbents to participate in the study of the recognition performance of the polymer.
[0029] The present invention will be further described below in conjunction with the accompanying drawings of the specific embodiment description.
[0030] Embodiment 1:
[0031] (1) Preparation of H-UiO-66-NH2
[0032] 110 mg of zirconium chloride, 1.82 g of benzoic acid, 180 mg of 2-aminoterephthalic acid and 146 mg of zinc nitrate hexahydrate were added to a 10 mL anhydrous N, N-dimethylformamide solution, ultrasonicated for 30 min, then transferred to a polytetrafluoroethylene reactor and reacted at 120 ° C for 24 h. The obtained product was collected by centrifugation and washed with DMF and anhydrous ethanol. The final product was added to 10 mL of pH = 1 hydrochloric acid solution and stirred for 15 minutes, then collected by centrifugation and washed with acetone, DMF and anhydrous ethanol in turn, and finally transferred to a vacuum oven and dried overnight at 60 ° C in vacuum to obtain mesoporous MOFs (H-UiO-66-NH2);
[0033] (2) Preparation of H-UiO-66-NH-Met
[0034] Disperse 50 mg of H-UiO-66-NH2 and 0.15 mmol of methyl methacrylate anhydride BMA in 4 mL of chloroform and heat at 55 °C for 24 hours, then centrifuge and soak in 14 mL of chloroform for three days, renew the solvent once a day, collect by centrifugation, and soak in 14 mL of methanol for three days, renew the solvent once a day. Collect by centrifugation, place, transfer to a vacuum oven, and dry at 150 °C for 2 hours to obtain H-UiO-66-NH-Met.
[0035] (3) Preparation of PBMMA-MOF-MIPs
[0036] 40 mg of H-UiO-66-NH-Met, 18 mg of acrylamidophenylboronic acid and 7 mg of naringin were suspended in 190 mg of butyl methacrylate (BMA) and sonicated for 20 minutes. 15 mg of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added to the mixture and sonicated for another 2 minutes. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV light for 12 h. Subsequently, 14 mL of eluent (methanol: acetic acid = 9:
[0037] 1) The template is eluted and air-dried to obtain the MOF-based boron affinity molecular imprinted membrane PBMMA-MOF-MIPs.
[0038] Non-imprinted polymers (PBMMA-MOF-NIPs) were prepared by the aforementioned protocol without the addition of NRG;
[0039] The blank flexible independent film was prepared without adding H-UiO-66-NH2-Met, acrylamidophenylboronic acid and naringin. 15 mg of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was directly added to 190 mg of butyl methacrylate (BMA) and ultrasonicated for another 2 minutes. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV lamp for 12 h.
[0040] from Figure 1 It can be seen that H-UiO-66-NH2 is in the shape of a sponge and has a porous structure on the surface, which is conducive to adsorption and mass transfer.
[0041] Depend on Figure 2 It can be seen that the H-UiO-66-NH-Met particles are uniformly dispersed within the membrane without voids at the interface, which indicates that the introduced polymerizable functional groups improve the chemical and physical interfacial interactions between MOF and polymer.
[0042] Depend on Figure 3 As shown, PBMMA-MOF-MIPs has a peak at 1354 cm -1 The BO absorption peak appeared at the bottom, indicating that the boric acid functionalized imprinted membrane was successfully prepared.
[0043] Depend on Figure 4 As shown, the XPS energy spectrum of PBMMA-MOF-MIPs. In the full spectrum (a), PBMMA-MOF-MIPs and PBMMA-MOF-NIPs have obvious absorption peaks of B, as well as the detailed spectrum analysis of B in (b).
[0044] Depend on Figure 5As shown in the EDS spectrum analysis of PBMMA-MOF-MIPs, two main characteristic peaks of B and Zr were detected, which proves that the boric acid functionalized MOFs imprinted membrane was successfully prepared.
[0045] Embodiment 2:
[0046] (1) Preparation of H-UiO-66-NH2
[0047] 120 mg of zirconium chloride, 1.83 g of benzoic acid, 181 mg of 2-aminoterephthalic acid and 148 mg of zinc nitrate hexahydrate were added to a 20 mL anhydrous N, N-dimethylformamide solution, ultrasonicated for 30 min, then transferred to a polytetrafluoroethylene reactor and reacted at 120 ° C for 24 h. The obtained product was collected by centrifugation and washed with DMF and anhydrous ethanol. The final product was added to 20 mL of pH = 1 hydrochloric acid solution and stirred for 15 minutes, then collected by centrifugation and washed with acetone, DMF and anhydrous ethanol in turn, and finally transferred to a vacuum oven and dried overnight at 60 ° C in vacuum to obtain mesoporous MOFs (H-UiO-66-NH2);
[0048] (2) Preparation of H-UiO-66-NH-Met
[0049] 60 mg of H-UiO-66-NH2 and 0.20 mmol of methyl methacrylate anhydride BMA were dispersed in 5 mL of chloroform and heated at 55 °C for 24 hours. Then, the mixture was centrifuged several times and soaked in 15 mL of chloroform for three days. The solvent was renewed every day. The mixture was collected by centrifugation and soaked in 15 mL of methanol for three days. The solvent was renewed every day. The mixture was collected by centrifugation and placed in a vacuum oven and dried at 150 °C for 2 hours to obtain H-UiO-66-NH-Met.
[0050] (3) Preparation of PBMMA-MOF-MIPs
[0051] 50 mg of H-UiO-66-NH-Met, 19 mg of acrylamidophenylboronic acid and 7.25 mg of naringin were suspended in 200 mg of butyl methacrylate (BMA) and sonicated for 20 min. 16 mg of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added to the mixture and sonicated for another 2 min. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV light for 12 h. Subsequently, the template was eluted in 15 mL of eluent (methanol: acetic acid = 9:1), and the MOF-based boron affinity molecular imprinted membrane PBMMA-MOF-MIPs was obtained after natural air drying.
[0052] The non-imprinted polymer (PBMMA-MOF-NIPs) was prepared by the aforementioned protocol without the addition of NRG; while the blank flexible independent membrane was prepared without the addition of H-UiO-66-NH2-Met, acrylamidophenylboronic acid and naringin. 16 mg of the photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was directly added to 200 mg of butyl methacrylate (BMA) and ultrasonicated for another 2 min. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV light for 12 h.
[0053] Embodiment 3:
[0054] (1) Preparation of H-UiO-66-NH2@BA
[0055] 130 mg of zirconium chloride, 1.84 g of benzoic acid, 182 mg of 2-aminoterephthalic acid and 148 mg of zinc nitrate hexahydrate were added to a 30 mL solution of anhydrous N,N-dimethylformamide, ultrasonicated for 30 min, and then transferred to a polytetrafluoroethylene reactor and reacted at 120 ° C for 24 h. The obtained product was collected by centrifugation and washed with DMF and anhydrous ethanol. The final product was added to 30 mL of pH = 1 hydrochloric acid solution and stirred for 15 minutes, then collected by centrifugation and washed with acetone, DMF and anhydrous ethanol in turn, and finally transferred to a vacuum oven and dried overnight at 60 ° C in vacuum to obtain boric acid functionalized MOFs (H-UiO-66-NH2@BA).
[0056] (2) Preparation of H-UiO-66-NH2-Met
[0057] 70 mg of H-UiO-66-NH2 and 0.25 mmol of methyl methacrylate anhydride BMA were dispersed in 6 mL of chloroform and heated at 55 °C for 24 hours. Then, the mixture was centrifuged several times and soaked in 16 mL of chloroform for three days. The solvent was renewed every day. The mixture was collected by centrifugation and soaked in 16 mL of methanol for three days. The solvent was renewed every day. The mixture was collected by centrifugation and placed in a vacuum oven and dried at 150 °C for 2 hours to obtain H-UiO-66-NH-Met.
[0058] (3) Preparation of PBMMA-MOF-MIPs
[0059] 60 mg of H-UiO-66-NH-Met, 20 mg of acrylamidophenylboronic acid and 7.5 mg of naringin were suspended in 210 mg of butyl methacrylate (BMA) and sonicated for 20 min. 17 mg of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added to the mixture and sonicated for another 2 min. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV light for 12 h. Subsequently, the template was eluted in 16 mL of eluent (methanol: acetic acid = 9:1), and the MOF-based boron affinity molecular imprinted membrane PBMMA-MOF-MIPs was obtained after natural air drying.
[0060] The non-imprinted polymer (PBMMA-MOF-NIPs) was prepared by the aforementioned protocol without the addition of NRG; while the blank flexible independent membrane was prepared without the addition of H-UiO-66-NH2-Met, acrylamidophenylboronic acid and naringin. 17 mg of the photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was directly added to 210 mg of butyl methacrylate (BMA) and ultrasonicated for another 2 min. The resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under UV light for 12 h.
[0061] Test Example 1:
[0062] Take 5.0mL of naringin (NRG) solution with an initial concentration of 35mg / L and add it to a centrifuge tube, add 5mg of the MOF-based boron affinity molecular imprinting flexible independent membrane adsorbent (PBMMA-MOF-MIPs) in Example 1, put the test solution in a water bath oscillator at 35°C, and take it out at 5min, 10min, 15min, 30min, 45min, 60min, 90min, 120min, and 180min respectively; separate the MOF-based boron affinity molecular imprinting flexible independent membrane adsorbent (PBMMA-MOF-MIPs) and naringin (NRG) solution, and then use a microporous nitrocellulose membrane with a pore size of 0.22mm to filter the solution to remove suspended particles. The NRG concentration in the filtrate is calculated and determined by an ultraviolet spectrophotometer at a wavelength of 283nm, and the adsorption capacity is calculated based on the results; from Figure 6 It can be concluded from the results that the adsorption process of PBMMA-MOF-MIPs can be divided into a rapid stage (the first 60 minutes) and a slow stage. The adsorption capacity of PBMMA-MOF-MIPs in the rapid stage reached 94.20% of the equilibrium capacity, and then slowly increased until equilibrium, proving the influence of the boric acid binding sites of the boron-affinity porous polymer on the adsorption. The boron-affinity porous polymer adsorbent is beneficial for the separation and enrichment of naringin molecules.
[0063] Test Example 2:
[0064] Take 5 mg of PBMMA-MOF-MIPs and add 5.0 mL of NRG solution (pH = 8.0) with initial concentrations of 5, 15, 25, 35 and 50 mg / L. Static adsorption was performed in a water bath for 3.0 h. The test solution was kept at 35 ° C. After the adsorption, the material was taken out and squeezed with tweezers, and the supernatant was taken. The NRG concentration in the squeezed liquid was detected by UV-vis, and the maximum absorption wavelength was 283 nm. The adsorption capacity was calculated based on the results. Figure 7 It can be concluded that when the initial concentration is 50 mg / L, the adsorption of MOF-based boron affinity molecular imprinted flexible independent membrane adsorbent (PBMMA-MOF-MIPs) tends to equilibrium.
[0065] Test Example 3:
[0066] Naringin, rutin, catechol, luteolin and hesperidin were selected as hydroxyl compounds for competitive adsorption, and aqueous solutions of the above four hydroxyl compounds were prepared respectively, and the concentration of each competitive adsorbent was 35 mg / L. 5 mL of the prepared solution was added to a centrifuge tube, and 5 mg of the MOF-based boron affinity molecular imprinted flexible independent membrane adsorbent (PBMMA-MOF-MIPs) in Example 1 was added respectively. The test solution was placed in a 35°C water bath and allowed to stand for 3.0 h. After the standing time was completed, the supernatant was collected by high-speed centrifugation, and the concentrations of various competitive adsorbed hydroxyl compounds that were not adsorbed were determined by ultraviolet. Figure 8 The results show that the adsorption capacity of PBMMA-MOF-MIPs for naringin, rutin, catechol, luteolin and hesperidin are 33.89; 7.25; 6.38; 9.36; 4.32 μmol / g, respectively. This shows that PBMMA-MOF-MIPs has significant recognition for NRG and its adsorption capacity is higher than that of other dihydroxy compounds.
Claims
1. A method for preparing a flexible MOFs-based boron affinity molecular imprinted membrane adsorbent, characterized in that: The steps include: (1) Prepare H-UiO-66-NH2 for later use; (2) Preparation of H-UiO-66-NH-Met, for later use; First, the H-UiO-66-NH2 prepared in step (1) and methacrylic anhydride are dispersed in a certain amount of chloroform A and heated for modification; then, the mixture is centrifuged and washed with chloroform for several times, and then, after being collected, it is immersed in a certain amount of chloroform B for a period of time, and the solvent is regularly renewed; after centrifugation and collection, it is immersed in a certain amount of methanol for a period of time, and the solvent is regularly renewed; finally, the mixture is centrifuged and placed, and then transferred to a vacuum oven for drying to obtain H-UiO-66-NH-Met; (3) Preparation of PBMMA-MOF-MIPs A certain amount of H-UiO-66-NH2-Met, acrylamidophenylboronic acid and naringin were suspended in a certain amount of butyl methacrylate BMA and ultrasonically treated; a certain amount of photoinitiator phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide was added to the mixture and ultrasonically treated, the resulting suspension was dropped into a polytetrafluoroethylene mold and photopolymerized under ultraviolet light; then, the template was eluted in a certain amount of eluent, and the MOF-based boron affinity molecular imprinting membrane PBMMA-MOF-MIPs was obtained after natural air drying.
2. The preparation method according to claim 1, characterized in that In step (1), the steps of preparing H-UiO-66-NH2 are as follows: adding a certain amount of zirconium chloride, benzoic acid, 2-aminoterephthalic acid and zinc nitrate hexahydrate to a certain amount of anhydrous N,N-dimethylformamide solution, ultrasonicating for 30 minutes; then transferring to a polytetrafluoroethylene reactor and reacting at 120°C for 24 hours, collecting the obtained product by centrifugation and washing it with DMF and anhydrous ethanol, adding a certain amount of hydrochloric acid solution with a pH of 1 and stirring for 15 minutes, then collecting it by centrifugation and washing it with acetone, DMF in sequence; and washed with anhydrous ethanol, and the collected product was transferred to a vacuum oven and dried overnight at 60°C in vacuum to obtain mesoporous MOFs, namely H-UiO-66-NH2; wherein the zirconium chloride, benzoic acid, 2-aminoterephthalic acid, zinc nitrate hexahydrate, anhydrous N,N-dimethylformamide, and hydrochloric acid solution were added in a ratio of (110-130) mg:(1.82-1.84) g:(180-182) mg:(146-150) mg:(10-30) mL:(10-30) mL.
3. The preparation method according to claim 1, characterized in that: In step (2), the usage ratio of H-UiO-66-NH2, methacrylic anhydride, chloroform A, chloroform B and methanol is (50-70) mg: (0.15-0.25) mmol: (4-6) mL: (14-16) mL: (14-16) mL.
4. The preparation method according to claim 1, characterized in that: In step (2), H-UiO-66-NH2 and methacrylic anhydride are dispersed in CHCl3 and heated at 55-60°C for 24 hours; immersed in chloroform for 3 days, and the same amount of solvent is replaced every day; immersed in methanol for 3 days, and the same amount of solvent is replaced every day; and vacuum drying conditions are 150°C for 2 hours.
5. The preparation method according to claim 1, characterized in that: In step (3), the amount ratio of H-UiO-66-NH-Met, acrylamidophenylboronic acid, naringin, butyl methacrylate BMA, photoinitiator phenyl bis (2,4,6-trimethylbenzoyl) phosphine oxide and eluent is (40-60) mg: (18-19) mg: (7-7.5) mg: (190-210) mg: (15-17) mg: (14-16) mL, wherein the eluent is a mixture of methanol and acetic acid, and the volume ratio of methanol: acetic acid is 9:
1.
6. The preparation method according to claim 1, characterized in that: In step (3), photopolymerization is carried out under ultraviolet light for 12 to 16 hours.
7. A flexible MOFs-based boron affinity molecular imprinted membrane adsorbent, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the flexible MOFs-based boron affinity molecular imprinted membrane adsorbent according to claim 7 for the selective separation of flavonoids.
9. The use according to claim 8, characterized in that Flexible MOFs-based boron affinity molecularly imprinted membrane adsorbent was used for the selective separation of o-dihydroxy compounds.