Black composite clay and preparation method thereof
By grinding and hydrothermal reaction of lignite, weathered coal, peat, grinding and hydrothermal reaction of nano-ferrous tetraoxide and sodium hydroxide, black composite clay was prepared, which solved the problem of low adhesion of water-based coatings and achieved excellent hydrophilicity It has antibacterial adsorption properties, suitable for water-based coating production, and has environmental protection and cost advantages.
Patent Information
- Application Number
- CN202310325023.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-03-30
AI Technical Summary
In actual applications, water-based coatings face problems such as long film formation time, low adhesion and easy cracking, which affects their wide application.
By crushing lignite, weathered coal, peat, mixing with nano iron tetraoxide and sodium hydroxide, and heat treatment in an air atmosphere, then adding hydrogen peroxide and sodium bentonite for hydrothermal reaction, it is sonicated and dried. Black bentonite/carbon dot/humidic acid composite clay was prepared.
The prepared black composite clay has natural black, excellent hydrophilic properties and dispersion, integrates good antibacterial and adsorption properties of carbon dots, humic acid and bentonite, and is used in the production of water-based coatings, overcoming the problem of low adhesion. It also has the advantages of green and environmental protection and low cost.
Smart Images

Figure CN116478563B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to black composite clay and a preparation method thereof, and belongs to the technical field of water-based paint production. Background Art
[0002] Waterborne paint is an organic polymer paint that uses water as a dispersion medium. During the coating process, the water gradually evaporates to form an organic polymer coating. Compared with organic solvent-based paints, waterborne paints have obvious advantages. During their production and use, they avoid releasing a large amount of volatile organic compounds (VOCs), which has less impact on the environment and human health. Therefore, they have attracted widespread attention in recent years. However, waterborne paints also face many technical difficulties in practical applications, such as long film formation time, low adhesion, and easy cracking. Solving these problems is of great significance for the widespread application of waterborne paints.
[0003] In view of this, it is necessary to propose a black composite clay and a preparation method thereof to solve the above problems. Summary of the invention
[0004] The object of the present invention is to provide a black composite clay and a preparation method thereof, which has the advantages of being green, environmentally friendly, low cost and wide applicability.
[0005] To achieve the above object, the present invention provides a method for preparing black composite clay, which mainly comprises the following steps:
[0006] Step 1, crushing one or more of lignite, weathered coal, and peat, then grinding and mixing the crushed lignite / weathered coal / peat with nano-ferroferric oxide and sodium hydroxide, performing heat treatment in an air atmosphere, and completing the pretreatment of the lignite / weathered coal / peat after cooling;
[0007] Step 2, adding hydrogen peroxide and sodium bentonite to the pretreated lignite / weathered coal / peat, keeping the mixture in a hydrothermal reactor for reaction, and performing solid-liquid separation after cooling to obtain a mixed liquid of black bentonite / carbon dots / sodium humate and a solid residue;
[0008] Step 3: Add additives to the mixed liquid of black bentonite / carbon dots / sodium humate obtained after separation, perform ultrasonic treatment, wash with water after cooling, and then dehydrate and dry to obtain bentonite / carbon dots / humic acid composite clay.
[0009] As a further improvement of the present invention, in step 1, the ground and mixed mixture is heat treated at 250-350° C. for 2-8 hours in an air atmosphere.
[0010] As a further improvement of the present invention, in step 1, the particle size of the nano-ferroferric oxide is 1-100 nanometers, the mass proportion of the nano-ferroferric oxide in the crushed lignite / weathered coal / peat is 0.1-5wt%, and the mass proportion of the sodium hydroxide in the crushed lignite / weathered coal / peat is 30-200wt%.
[0011] As a further improvement of the present invention, in step 2, the concentration of the hydrogen peroxide is 2-30wt%, the mass proportion of the hydrogen peroxide in the pretreated lignite / weathered coal / peat is 100-500wt%, and the mass proportion of the sodium bentonite in the pretreated lignite / weathered coal / peat is 20-200wt%.
[0012] As a further improvement of the present invention, in step 2, the reaction is carried out in a hydrothermal kettle at 100-150° C. for 2-4 hours.
[0013] As a further improvement of the present invention, in step 2, the pH value of the solid residue is adjusted to 6-7, and the solid residue is dried.
[0014] As a further improvement of the present invention, in step 3, ultrasonic treatment is performed at 40-100° C. for 2-4 hours.
[0015] As a further improvement of the present invention, in step 3, the additive is one or more of hexadecyltrimethylammonium bromide, stearic acid, and polyether polyol, and the mass proportion of the additive in the mixed liquid of black bentonite / carbon dots / sodium humate is 1-5wt%.
[0016] To achieve the above object, the present invention further provides a black composite clay, which is prepared using the above-mentioned method for preparing the black composite clay.
[0017] As a further improvement of the present invention, the black composite clay includes bentonite, carbon dots and humic acid composite clay, wherein the mass ratio of the bentonite, the carbon dots and the humic acid composite clay is 1:0.01-0.15:0.2-5.
[0018] The beneficial effects of the present invention are as follows: the black composite clay prepared by the present invention has natural black color, excellent hydrophilicity and dispersibility, and integrates the good antibacterial and adsorption properties of carbon dots, humic acid and bentonite, and can be used for the production of water-based coatings. It also has the advantages of being green, environmentally friendly, and low-cost, and has wide applicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a photo of the bentonite / carbon dots / humic acid composite clay obtained in Example 1.
[0020] Figure 2The antibacterial effect of the bentonite / carbon dots / humic acid composite clay obtained in Example 1 on Staphylococcus aureus is shown in Figure 1, where A is the blank group and B is the group after adding the composite clay. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0022] It should be noted here that in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.
[0023] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0024] like Figure 1 and Figure 2 As shown, the present invention discloses a black composite clay and a preparation method thereof, wherein lignite / weathered coal / peat is pretreated, and then hydrogen peroxide and sodium bentonite are added, and bentonite / carbon dots / humic acid composite clay is obtained after hydrothermal catalytic oxidation, separation, modification, and drying steps. The black composite clay comprises bentonite, carbon dots, and humic acid composite clay, wherein the mass ratio of the bentonite, the carbon dots, and the humic acid composite clay is 1:0.01-0.15:0.2-5.
[0025] The preparation method of the black composite clay mainly comprises the following steps:
[0026] Step 1, crushing one or more of lignite, weathered coal, and peat, then grinding and mixing the crushed lignite / weathered coal / peat with nano-ferroferric oxide and sodium hydroxide, performing heat treatment in an air atmosphere, and completing the pretreatment of the lignite / weathered coal / peat after cooling;
[0027] Step 2, adding hydrogen peroxide and sodium bentonite to the pretreated lignite / weathered coal / peat, keeping the mixture in a hydrothermal reactor for reaction, and performing solid-liquid separation after cooling to obtain a mixed liquid of black bentonite / carbon dots / sodium humate and a solid residue;
[0028] Step 3: Add additives to the mixed liquid of black bentonite / carbon dots / sodium humate obtained after separation, perform ultrasonic treatment, wash with water after cooling, and then dehydrate and dry to obtain bentonite / carbon dots / humic acid composite clay.
[0029] Steps 1 to 3 are described in detail below.
[0030] In step 1, the mixture of lignite / weathered coal / peat, nano-ferroferric oxide and sodium hydroxide after grinding and mixing is heat-treated at 250-350° C. for 2-8 hours in an air atmosphere.
[0031] The particle size of the nano-ferroferric oxide is 1-100 nanometers, the mass proportion of the nano-ferroferric oxide in the crushed lignite / weathered coal / peat is 0.1-5wt%, and the mass proportion of the sodium hydroxide in the crushed lignite / weathered coal / peat is 30-200wt%.
[0032] In step 2, the concentration of the hydrogen peroxide is 2-30wt%, the mass proportion of the hydrogen peroxide in the pretreated lignite / weathered coal / peat is 100-500wt%, and the mass proportion of the sodium bentonite in the pretreated lignite / weathered coal / peat is 20-200wt%. Hydrogen peroxide and sodium bentonite are added to the pretreated lignite / weathered coal / peat, and the reaction needs to be kept in a hydrothermal autoclave at 100-150°C for 2-4 hours.
[0033] It should be noted that, by adjusting the pH value of the solid residue to 6-7 and drying the solid residue, a soil conditioner that can be used for saline-alkali land treatment is obtained.
[0034] In step 3, the additive is one or more of hexadecyltrimethylammonium bromide, stearic acid, and polyether polyol, and the mass proportion of the additive in the mixed liquid of black bentonite / carbon dots / sodium humate is 1-5wt%. After the additive is added, the mixed liquid is ultrasonically treated at 40-100°C for 2-4 hours.
[0035] The following is a detailed description with reference to the embodiments.
[0036] Embodiment 1 specifically comprises the following steps:
[0037] The weathered coal is pretreated by crushing the weathered coal, then the crushed weathered coal is ground and mixed with 2wt% of nano-ferroferric oxide (size 1-100 nanometers) and 100wt% of sodium hydroxide, and then the mixture is heat-treated at 350°C for 2 hours in an air atmosphere, and the pretreatment of the weathered coal is completed after cooling. Then, 300wt% of 10wt% hydrogen peroxide and 100wt% of sodium bentonite are added, and the mixture is kept warm at 120°C in a hydrothermal reactor for 2 hours, and solid-liquid separation is performed after cooling to obtain a black bentonite / carbon point / sodium humate mixed liquid and solid residue.
[0038] The pH value of the solid residue is adjusted to 7, and after drying, a soil conditioner that can be used for saline-alkali land treatment is obtained; 2wt% of hexadecyltrimethylammonium bromide additive is added to the black bentonite / carbon dots / sodium humate mixed liquid obtained after separation, and ultrasonic treatment is performed at 70°C for 3 hours. After cooling, the mixture is washed with water, and then dehydrated and dried to obtain bentonite / carbon dots / humic acid composite clay.
[0039] In this embodiment, the prepared bentonite / carbon dot / humic acid composite clay was tested for hue, dispersion, adhesion, antibacterial and adsorption properties. The results showed that its hue was black with a reddish tint; after 5 hours of oscillation, the fineness of the paint particles in the color paste was less than 5 microns and was well dispersed; the coating adhesion was not less than 9.5 N / cm2; the minimum inhibitory concentrations MIC for Staphylococcus aureus and Escherichia coli were 0.03 mg / L and 0.12 mg / L, respectively; and the adsorption removal rate of formaldehyde reached 95.1%.
[0040] Embodiment 2 specifically comprises the following steps:
[0041] The peat is pretreated by crushing it, then grinding and mixing the crushed peat with 1wt% of nano-ferroferric oxide (size 1-100 nanometers) and 100wt% of sodium hydroxide, and then heat-treating the mixture at 350°C for 2 hours in an air atmosphere, and completing the pretreatment of the peat after cooling. Then, 400wt% of 10wt% hydrogen peroxide and 100wt% sodium bentonite are added, and the mixture is kept warm at 120°C in a hydrothermal reactor for 2 hours, and solid-liquid separation is performed after cooling to obtain a black bentonite / carbon point / sodium humate mixed liquid and a solid residue.
[0042] The pH value of the solid residue is adjusted to 7, and after drying, a soil conditioner that can be used for saline-alkali land treatment is obtained; 2wt% of a polyether polyol additive is added to the black bentonite / carbon dot / sodium humate mixed liquid obtained after separation, and the mixture is ultrasonically treated at 70°C for 3 hours, washed with water after cooling, and then dehydrated and dried to obtain a bentonite / carbon dot / humic acid composite clay.
[0043] In this embodiment, the prepared bentonite / carbon dot / humic acid composite clay was tested for hue, dispersion, adhesion, antibacterial and adsorption properties. The results showed that its hue was black with a reddish tint; after 5 hours of oscillation, the fineness of the paint particles in the color paste was less than 7 microns and was well dispersed; the coating adhesion was not less than 9.5 N / cm2; the minimum inhibitory concentrations MIC for Staphylococcus aureus and Escherichia coli were 0.04 mg / L and 0.15 mg / L, respectively; and the adsorption removal rate of formaldehyde reached 96.3%.
[0044] Embodiment 3 specifically comprises the following steps:
[0045] The peat is pretreated by crushing it, then grinding and mixing the crushed peat with 1wt% of nano-ferroferric oxide (size 1-100 nanometers) and 100wt% of sodium hydroxide, and then heat-treating the mixture at 350°C for 2 hours in an air atmosphere, and completing the pretreatment of the peat after cooling. Then, 400wt% of 10wt% hydrogen peroxide and 80wt% of sodium bentonite are added, and the mixture is kept warm at 120°C in a hydrothermal reactor for 2 hours, and solid-liquid separation is performed after cooling to obtain a black bentonite / carbon point / sodium humate mixed liquid and a solid residue.
[0046] The pH value of the solid residue is adjusted to 7, and after drying, a soil conditioner that can be used for saline-alkali land treatment is obtained; 3wt% of a stearic acid additive is added to the black bentonite / carbon dots / sodium humate mixed liquid obtained after separation, and the mixture is ultrasonically treated at 70°C for 3 hours, and washed with water after cooling, and then dehydrated and dried to obtain a bentonite / carbon dots / humic acid composite clay.
[0047] In this embodiment, the prepared bentonite / carbon dot / humic acid composite clay was tested for hue, dispersion, adhesion, antibacterial and adsorption properties. The results showed that its hue was black with a reddish tint; after 5 hours of oscillation, the fineness of the paint particles in the color paste was less than 7 microns and was well dispersed; the coating adhesion was not less than 9.4 N / cm2; the minimum inhibitory concentrations MIC for Staphylococcus aureus and Escherichia coli were 0.03 mg / L and 0.14 mg / L, respectively; and the adsorption removal rate of formaldehyde reached 97.2%.
[0048] Embodiment 4 specifically comprises the following steps:
[0049] The lignite is pretreated and crushed, and then the crushed lignite is ground and mixed with 1wt% of nano-ferroferric oxide (size 1-100 nanometers) and 100wt% of sodium hydroxide, and then the mixture is heat-treated at 350°C for 2 hours in an air atmosphere, and the pretreatment of the lignite is completed after cooling. Then, 400wt% of 10wt% hydrogen peroxide and 80wt% of sodium bentonite are added, and the mixture is kept warm at 120°C in a hydrothermal autoclave for 2 hours, and solid-liquid separation is performed after cooling to obtain a black bentonite / carbon point / sodium humate mixed liquid and a solid residue.
[0050] The pH value of the solid residue is adjusted to 7, and after drying, a soil conditioner that can be used for saline-alkali land treatment is obtained; 3wt% of hexadecyltrimethylammonium bromide and stearic acid additives of equal mass are added to the black bentonite / carbon dots / sodium humate mixed liquid obtained after separation, and ultrasonic treatment is performed at 70°C for 3 hours. After cooling, the mixture is washed with water, and then dehydrated and dried to obtain bentonite / carbon dots / humic acid composite clay.
[0051] In this embodiment, the prepared bentonite / carbon dot / humic acid composite clay was tested for hue, dispersion, adhesion, antibacterial and adsorption properties. The results showed that its hue was black with a reddish tint; after 5 hours of oscillation, the fineness of the paint particles in the color paste was less than 8 microns and was well dispersed; the coating adhesion was not less than 9.5 N / cm2; the minimum inhibitory concentrations MIC for Staphylococcus aureus and Escherichia coli were 0.05 mg / L and 0.13 mg / L, respectively; and the adsorption removal rate of formaldehyde reached 96.7%.
[0052] The performance test results of the bentonite / carbon dots / humic acid composite clay in each embodiment are shown in Table 1 below.
[0053] Table 1 Performance test results of bentonite / carbon dots / humic acid composite clay in each embodiment
[0054]
[0055] In summary, it can be further seen from Examples 1-4 that the organic composite clay provided by the present invention has natural black color, good hydrophilicity and dispersibility, overcomes the disadvantage of low adhesion of conventional water-based coatings, and integrates the good antibacterial and adsorption properties of carbon dots, humic acid and bentonite, and can be used for the production of water-based coatings. It also has the advantages of being green, environmentally friendly, low cost, and wide applicability.
[0056] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for preparing black composite clay, characterized in that: The main steps include: Step 1, crushing one or more of lignite, weathered coal, and peat, then grinding and mixing the crushed lignite / weathered coal / peat with nano-ferroferric oxide and sodium hydroxide, heat-treating the ground mixture at 250-350° C. for 2-8 hours in an air atmosphere, and completing the pretreatment of the lignite / weathered coal / peat after cooling; Step 2, adding hydrogen peroxide and sodium bentonite to the pretreated lignite / weathered coal / peat, keeping the mixture in a hydrothermal reactor for reaction, and performing solid-liquid separation after cooling to obtain a mixed liquid of black bentonite / carbon dots / sodium humate and a solid residue; Step 3, adding additives to the mixed liquid of black bentonite / carbon dots / sodium humate obtained after separation, performing ultrasonic treatment, washing with water after cooling, and then dehydrating and drying to obtain bentonite / carbon dots / humic acid composite clay; Wherein, in step 1, the particle size of the nano-ferroferric oxide is 1-100 nanometers, the mass proportion of the nano-ferroferric oxide in the crushed lignite / weathered coal / peat is 0.1-5wt%, and the mass proportion of the sodium hydroxide in the crushed lignite / weathered coal / peat is 30-200wt%; In step 2, the concentration of the hydrogen peroxide is 2-30wt%, the mass proportion of the hydrogen peroxide in the pretreated lignite / weathered coal / peat is 100-500wt%, and the mass proportion of the sodium bentonite in the pretreated lignite / weathered coal / peat is 20-200wt%.
2. The method for preparing black composite clay according to claim 1, characterized in that: In step 2, the reaction is carried out in a hydrothermal reactor at 100-150° C. for 2-4 hours.
3. The method for preparing black composite clay according to claim 1, characterized in that: In step 2, the pH value of the solid residue is adjusted to 6-7, and the solid residue is dried.
4. The method for preparing black composite clay according to claim 1, characterized in that: In step 3, ultrasonic treatment is performed at 40-100°C for 2-4 hours.
5. The method for preparing black composite clay according to claim 1, characterized in that: In step 3, the additive is one or more of cetyltrimethylammonium bromide, stearic acid, and polyether polyol, and the mass proportion of the additive in the mixed liquid of black bentonite / carbon dots / sodium humate is 1-5wt%.
6. A black composite clay, characterized in that: The method for preparing the black composite clay is used as described in any one of claims 1 to 5.
7. The black composite clay according to claim 6, characterized in that: The black composite clay comprises bentonite, carbon dots and humic acid composite clay, wherein the mass ratio of the bentonite, the carbon dots and the humic acid composite clay is 1:0.01-0.15:0.2-5.