Preparation method and application of Dy2O3 / ultra-thin graphite phase carbon nitride composite material

By preparing Dy2O3/ultrathin graphite phase carbon nitride composite optical probe, the problems of complicated preparation process and poor stability of cysteine ​​electrochemiluminescence probe in the existing technology are solved, achieving high sensitivity and high selectivity. Quantitative detection, and the material has good biocompatibility and stability.

CN116495765BActive Publication Date: 2024-10-22ANHUI UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310476265.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-22
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

The preparation process of existing cysteine ​​electrochemiluminescence probes is complicated, the reaction conditions are harsh, the raw materials are rare, and the purification and separation processes are difficult, resulting in poor sensing sensitivity and selectivity, and the inability to quantitatively detect, and the probes are repeatedly reusable and stable. Not strong.

Method used

Through simple solid-state thermal reaction steps and mild reaction conditions, an environmentally friendly and non-toxic Dy2O3/ultrathin graphite phase carbon nitride composite optical probe was prepared and modified with a glassy carbon electrode to significantly enhance the electrochemiluminescence signal. A new system for quantitative detection of cysteine.

Benefits of technology

It achieves high-sensitivity and high-selectivity identification and quantitative detection of cysteine. The material has good biocompatibility, reproducibility and long-term stability, and reduces raw material prices and preparation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116495765B_ABST
    Figure CN116495765B_ABST
Patent Text Reader

Abstract

The invention discloses a Dy 2 O 3 / The preparation method and application of ultra-thin graphite phase carbon nitride composite materials belong to the field of inorganic material synthesis technology. The material first uses acetone to treat urea, and then calcines to obtain ultra-thin g-C 3 N 4 Then, ultra-thin g‑C 3 N 4 and Dy(NO 3 ) 3 •6H 2 O, after ultrasonic dispersion, stirring reaction for a period of time, finally the dried precursor is placed in a muffle furnace for calcination, and the target product is obtained after annealing. The raw materials of the composite material are cheap and easy to obtain, the preparation process is simple, and a green and pollution-free solvent is used. The prepared material has excellent biocompatibility, conductivity and photoelectrocatalytic activity, which is manifested in that the composite material is dispersed and immobilized on a substrate glassy carbon electrode, and can be successfully used for electrochemiluminescence response to cysteine, the amount of modifier used is extremely small, and the response sensitivity, specific selectivity, stability and reversibility are good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of inorganic material synthesis and relates to a Dy 2 O 3 / Preparation method and application of ultra-thin graphite phase carbon nitride composite material, specifically, a Dy 2 O 3 / Ultra-thin graphite carbon nitride (gC 3 N 4 ) Preparation method of composite material. Background Art

[0002] Cysteine ​​(Cys) is the only amino acid containing sulfur in biological cells. It plays an important role in physiological processes such as protein synthesis, metabolism, and detoxification. It can participate in many redox processes in cells and phospholipid metabolism in the liver. At the same time, cysteine ​​also has the function of protecting liver cells from damage and promoting liver function recovery. In normal cells of organisms, cysteine ​​is maintained in a certain range of 30-200μmol / L. Abnormal concentrations will increase the probability of diseases such as liver damage, growth retardation, muscle atrophy, cardiovascular disease and even cancer. Therefore, it is very important to detect the actual content of cysteine ​​in organisms. Among the many methods for detecting cysteine, the electrochemiluminescence method, which does not require an external light source, has high photostability and sensitivity, a wide linear range, and low background interference, stands out.

[0003] Graphene carbon nitride (gC nitride) is a kind of carbon nitride with low cost, easy preparation, good physical and chemical stability, non-toxicity and unique electronic structure. 3 N 4 ) is an important indirect semiconductor material, widely used in catalysis, optoelectronic materials, sensors and environmental remediation. 3 N 4 It is a block or layered structure. Due to the interaction between adjacent CN layers, its visible light utilization rate and conductivity are low. Inspired by graphene research, researchers have carried out ultra-thin gC 3 N 4 In order to further broaden the scope of gC 3 N 4 One of the approaches that has attracted much attention at present is to improve its light absorption range in the visible light region, compensate for its light capture ability, inhibit the recombination of photogenerated electron and hole pairs, and improve its photoelectric application efficiency by combining with semiconductors.

[0004] Dysprosium oxide (Dy) is a rare earth oxide with abundant reserves, special electronic structure and energy level, good chemical stability and thermal stability. 2 O 3) was once used to construct an electrochemical sensor to detect nitrite, and gold nanomaterials (AuNPs) modified Dy 2 O 3 These studies have shown that Dy 2 O 3 Excellent electrocatalytic performance.

[0005] Ultra-thin gC 3 N 4 The substrate is reacted with Dy 2 O 3 Composite preparation of new composite materials, synergistically exerting ultra-thin gC 3 N 4 Visible light utilization, conductivity and Dy 2 O 3 The electrocatalytic performance of cysteine ​​was improved by constructing a new electrochemiluminescence system that responds to cysteine, which is expected to improve the defects of traditional cysteine ​​electrochemiluminescence probes, such as expensive raw materials, cumbersome synthesis steps, harsh reaction conditions, low probe molecular sensing sensitivity, weak recognition selectivity, poor biocompatibility, and poor probe stability. It effectively broadens the application of rare earth oxides and ultrathin gC 3 N 4 The application field of the material provides a theoretical research basis for the design and preparation of efficient and sensitive electrochemiluminescence sensors. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art, such as the complicated preparation process of electrochemiluminescent probes, the difficulty in implementing reaction conditions, the difficulty in obtaining raw materials, the difficulty in purification and separation, the low loading amount of the target resulting in poor sensing sensitivity and selectivity, the inability to quantitatively detect, the low probe reuse rate and stability, etc., and to prepare and separate environmentally friendly, non-toxic and excellent performance Dy through simple solid-phase thermal reaction steps and mild reaction conditions. 2 O 3 / Ultra-thin gC 3 N 4 Composite optical probes enable cysteine ​​to interact with trace amounts of Dy modified on glassy carbon electrodes in a green, pollution-free aqueous testing environment. 2 O 3 / Ultra-thin gC 3 N 4 The composite material exhibits significant changes in electrochemiluminescence signals, thus establishing a new system for the quantitative detection of cysteine. The study also found that common coexisting substances have almost no effect on the measurement results, thus demonstrating the composite material's ability to highly sensitively and selectively identify and quantitatively detect cysteine.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A kind of Dy 2 O 3 / A method for preparing an ultra-thin graphite phase carbon nitride composite material comprises the following steps:

[0009] The first step is to use a certain amount of acetone to pre-treat urea for a certain period of time, remove the solvent, and then heat and calcine in a muffle furnace to obtain ultra-thin gC 3 N 4 ;

[0010] Step 2: Add weighed Dy(NO 3 ) 3 •6H 2 O and ultrathin gC prepared by the first step reaction 3 N 4 , ultrasonic dispersion is used to form a uniform dispersion of the two in water, and then a certain temperature is set to stir the reaction;

[0011] The third step is to centrifuge the material obtained in the previous step, wash it with ultrapure water, and then dry it in an oven;

[0012] Step 4: Finally, the dried precursor is placed in a crucible and placed in a muffle furnace to be calcined at a certain temperature for a period of time. After annealing, the target product Dy 2 O 3 / Ultra-thin gC 3 N 4 Composite materials.

[0013] Furthermore, in the first step, the dosage ratio of acetone to urea is 60-80 mL:8-15 g.

[0014] Furthermore, in the first step, the pretreatment time is 2-4 h, and the muffle furnace calcination parameters are: calcination at 450-650° C. for 3-6 h.

[0015] Furthermore, in the second step, ultrapure water, ultrathin gC 3 N 4 and Dy(NO 3 ) 3 •6H 2 The dosage ratio of O is 10-20 mL:200 mg:8-32 mg.

[0016] Furthermore, in the second step, the ultrasonic dispersion time is 8-15 min; the stirring reaction parameters are: temperature 65-75°C, time 4-8 h.

[0017] Furthermore, in the third step, the oven drying parameters are: drying at 70-90° C. for 1-3 h.

[0018] Furthermore, in the fourth step, the muffle furnace calcination parameters are: heating at a rate of 5°C / min to 450-650°C for 3-6 h.

[0019] The composite material prepared above is used in electrochemiluminescence sensing and quantitative detection of cysteine. Cysteine ​​can be used in ultrathin gC 3 N 4 Dy 2 O 3 The electrochemiluminescence signal of the composite material is significantly enhanced, thereby utilizing the sensitization effect to construct a new type of electrochemiluminescence sensing probe.

[0020] The ultra-thin graphene-like carbon nitride (gC N2) with low raw material cost, simple preparation, environmental protection and non-toxicity, large specific surface area, high chemical stability and further improved electrical conductivity is used. 3 N 4 ) as the base material and dysprosium oxide, one of the rare earth oxides with abundant reserves, unique energy band structure and excellent electrocatalytic performance, to prepare a new composite material. The study found that because the composite material exerts ultra-thin gC 3 N 4 The synergistic effect between the composite material and dysprosium oxide promotes electron migration, improves luminescence efficiency and biocompatibility, and increases the number of active sites and sample loading rate on the surface of the electrochemiluminescence sensor modified electrode constructed by the composite material, resulting in a significant inhibitory effect of the target cysteine ​​in the system on the electrochemiluminescence signal of the composite material modified electrode, and finally a new system for responding to and detecting cysteine ​​in the aqueous phase was established. The sensor constructed by the composite material has high sensitivity, strong selectivity, good reproducibility and long-term stability, and can be developed for specific recognition and trace detection of cysteine ​​in organisms, promoting the application prospects of graphite phase carbonized nitrogen and rare earth oxide materials in the field of biosensing.

[0021] Beneficial effects of the present invention:

[0022] 1. The raw materials are cheap and the preparation process is simple;

[0023] 2. The reaction conditions are relatively mild, saving energy and reducing consumption;

[0024] 3. The prepared composite material has good biocompatibility, and the subsequent testing solvent is environmentally friendly and friendly to humans and the environment;

[0025] 4. The solid-phase electrochemiluminescence method is used to respond to cysteine, which not only requires less probe, but also has high sensitivity and good specificity;

[0026] 5. It can realize the quantitative detection of trace cysteine;

[0027] 6. The probe material has excellent reproducibility and good stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The present invention will be further described below in conjunction with the accompanying drawings.

[0029] Figure 1 For the present invention Dy 2 O 3 / Ultra-thin gC 3 N 4 Preparation process of the composite material (DUCN) and its electrochemiluminescence response to cysteine.

[0030] Figure 2 For ultra-thin gC 3 N 4 (UCN), Dy 2 O 3 And Dy prepared in Example 3 of the present invention 2 O 3 / Ultra-thin gC 3 N 4 X-ray powder diffraction pattern (A) and transmission electron microscopy (B) of the composite material (DUCN) (a in B is the ultra-thin gC 3 N 4 , b is Dy 2 O 3 Nanoparticles, c is Dy 2 O 3 / Ultra-thin gC 3 N 4 composite materials).

[0031] Figure 3 Ultrathin gC in PBS (0.1 M pH = 7) buffer solution 3 N 4 (UCN) modified glassy carbon electrode (UCN / GCE), Dy 2 O 3 Modified glassy carbon electrode (Dy 2 O 3 / GCE), Dy prepared in Example 3 of the present invention 2 O 3 / Ultra-thin gC 3 N 4 Composite material modified glassy carbon electrode (DUCN / GCE) and Dy after adding cysteine 2 O 3 / Ultra-thin gC 3 N 4 Electrochemiluminescence behavior of composite material modified glassy carbon electrode (DUCN / GCE).

[0032] Figure 4 Dy prepared in Example 3 of the present invention 2 O3 / Ultra-thin gC 3 N 4 ECL response curves of composite material modified glassy carbon electrode (DUCN / GCE) to different concentrations of cysteine.

[0033] Figure 5 The effect of an equal amount of cysteine ​​and possible coexisting substances on the Dy prepared in Example 3 of the present invention 2 O 3 / Ultra-thin gC 3 N 4 Effect of composite materials modified glassy carbon electrode (DUCN / GCE) on electrochemiluminescence signal. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The ultra-thin gC used in the present invention 3 N 4 It was prepared by thermal polycondensation with acetone pretreatment, referring to relevant materials (Jiang L, Li J, Wang K, Zhang G, Li Y, Wu X. Low boiling point solventmediated strategy to synthesize functionalized monolayer carbon nitride forsuperior photocatalytic hydrogen evolution. Applied Catalysis B:Environmental, 2020, 260:118181-118190.)

[0036] The composite materials in the examples were characterized by an X-ray powder diffractometer model D8 ADVANCE from Bruker, Germany, and a transmission electron microscope model HT-7700 from Hitachi, Japan; the electrochemiluminescence test was performed by an MPI-B electrochemiluminescence analyzer from Xi'an Ruimai Analytical Instrument Co., Ltd. and a three-electrode system, i.e., a glassy carbon electrode (GCE, Ø = 3 mm) or a composite material-modified glassy carbon electrode as the working electrode, Ag / AgCl as the reference electrode, and a platinum wire as the counter electrode.

[0037] Figure 1 The Dy2 O 3 / Ultra-thin gC 3 N 4 Preparation process of the composite material (DUCN) and its electrochemiluminescence response to cysteine.

[0038] Example 1

[0039] (1) Weigh 8 g of urea and dissolve it in 60 mL of acetone. Stir it at room temperature for 2 h. After standing for 8 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and calcine it at 450 °C at a heating rate of 5 °C / min for 6 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0040] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4 Then, 12 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 10 min to form a uniform dispersion in water. The mixture was stirred and reacted at 70 °C for 6 h.

[0041] (3) The product was separated by centrifugation and washed with ultrapure water for three times, and then dried in an oven at 70°C for 3 h.

[0042] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 550°C for 4 h at a heating rate of 5°C / min. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0043] Example 2

[0044] (1) Weigh 15 g of urea and dissolve it in 80 mL of acetone. Stir it at room temperature for 4 h. After standing for 15 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and calcine it at 650 °C at a heating rate of 5 °C / min for 3 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0045] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4Then, 16 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 10 min to form a uniform dispersion in water. The mixture was stirred and reacted at 70 °C for 6 h.

[0046] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 90°C for 1 h.

[0047] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 550°C at a heating rate of 5°C / min for 5 h. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0048] Example 3

[0049] (1) Weigh 10 g of urea and dissolve it in 70 mL of acetone. Stir it at room temperature for 3 h. After standing for 10 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 550 °C at a rate of 5 °C / min for 5 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0050] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4 Then, 24 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 10 min to form a uniform dispersion in water. The mixture was stirred and reacted at 70 °C for 6 h.

[0051] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 85°C for 2 h.

[0052] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 550°C for 4 h at a heating rate of 5°C / min. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0053] Example 4

[0054] (1) Weigh 10 g of urea and dissolve it in 70 mL of acetone. Stir it at room temperature for 3 h. After standing for 10 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 550 °C at a rate of 5 °C / min for 5 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0055] (2) First, add 200 mg of the ultrathin gC prepared above into 10 mL of ultrapure water. 3 N 4 Then, 8 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 8 min to form a uniform dispersion in water. The mixture was stirred and reacted at 65 °C for 8 h.

[0056] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 85°C for 2 h.

[0057] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 550°C for 4 h at a heating rate of 5°C / min. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0058] Example 5

[0059] (1) Weigh 10 g of urea and dissolve it in 70 mL of acetone. Stir it at room temperature for 3 h. After standing for 10 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 550 °C at a rate of 5 °C / min for 5 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0060] (2) First, add 200 mg of the ultrathin gC prepared above into 20 mL of ultrapure water. 3 N 4 Then, 32 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 15 min to form a uniform dispersion in water. The mixture was stirred and reacted at 75 °C for 4 h.

[0061] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 85°C for 2 h.

[0062] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 550°C for 4 h at a heating rate of 5°C / min. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0063] Example 6

[0064] (1) Weigh 10 g of urea and dissolve it in 70 mL of acetone. Stir it at room temperature for 3 h. After standing for 10 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 550 °C at a rate of 5 °C / min for 5 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0065] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4 Then, 28 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 15 min to form a uniform dispersion in water. The mixture was stirred and reacted at 70 °C for 6 h.

[0066] (3) The product was separated by centrifugation and washed with ultrapure water for three times, and then dried in an oven at 70°C for 3 h.

[0067] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 450°C at a heating rate of 5°C / min for 6 h. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0068] Example 7

[0069] (1) Weigh 10 g of urea and dissolve it in 70 mL of acetone. Stir it at room temperature for 3 h. After standing for 10 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 550 °C at a rate of 5 °C / min for 5 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0070] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4 Then, 24 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 12 min to form a uniform dispersion in water. The mixture was stirred and reacted at 70 °C for 6 h.

[0071] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 90°C for 1 h.

[0072] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 650°C at a heating rate of 5°C / min for 3 h. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0073] Example 8

[0074] (1) Weigh 12 g of urea and dissolve it in 75 mL of acetone. Stir it at room temperature for 3 h. After standing for 12 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 500 °C at a rate of 5 °C / min for 4 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0075] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4 Then, 12 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 12 min to form a uniform dispersion in water. The mixture was stirred and reacted at 80 °C for 5 h.

[0076] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 85°C for 2 h.

[0077] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and calcined at 550°C for 4 h at a heating rate of 5°C / min. After annealing, Dy 2 O 3 / Ultra-thin gC3 N 4 The composite material is labeled as DUCN.

[0078] Example 9

[0079] (1) Weigh 15 g of urea and dissolve it in 80 mL of acetone. Stir it at room temperature for 4 h. After standing for 12 min, remove the solvent. Then, place the crucible containing the pre-treated urea in a muffle furnace and heat it to 600 °C at a rate of 5 °C / min for 5 h. After annealing, ultrathin gC 3 N 4 The product is labeled UCN.

[0080] (2) First, add 200 mg of the ultrathin gC prepared above into 15 mL of ultrapure water. 3 N 4 Then, 20 mg of Dy(NO 3 ) 3 •6H 2 O was added to the above solution and ultrasonically dispersed for 12 min to form a uniform dispersion in water. The mixture was stirred and reacted at 75 °C for 6 h.

[0081] (3) The product was separated by centrifugation and washed with ultrapure water three times, and then dried in an oven at 80°C for 2 h.

[0082] (4) The dried precursor was placed in a crucible and placed in a muffle furnace and heated to 500°C for 5 h at a rate of 5°C / min. After annealing, Dy 2 O 3 / Ultra-thin gC 3 N 4 The composite material is labeled as DUCN.

[0083] Evaluation of the electrochemiluminescence recognition and detection effect of the composite material prepared in the above embodiment on cysteine

[0084] The Dy prepared in the best embodiment 3 was characterized by X-ray powder diffractometer and transmission electron microscope. 2 O 3 / Ultra-thin gC 3 N 4 The physical phase and morphology of the composite material (DUCN) were investigated. Then 2 mg of the prepared composite optical probe was ultrasonically dispersed in 2 mL of a mixed solvent of water and ethanol containing 6 μL of Nafion solution. Then 2 μL of the solution was drop-coated on the surface of the glassy carbon electrode. After drying, a sensor was constructed to study its electrochemiluminescence response to cysteine.

[0085] (1) In the experiment, the prepared materials were first characterized by X-ray powder diffractometer (XRD). The results are as follows: Figure 2 As shown in A. 2 O 3 / Ultra-thin gC 3 N 4 The composite material has two prominent diffraction peaks at 13.0° and 27.5°, just like UCN, which correspond to the periodic stacking (100) crystal plane between the layers in the graphite structure of the UCN material and the (002) crystal plane reflecting the interlayer stacking reflection of its conjugated aromatic system. The DUCN composite material faintly appears at 43.7° and 57.2°, respectively, which is similar to the single Dy prepared in the present invention. 2 O 3 Nanomaterials and Dy Simulation 2 O 3 The diffraction peaks of the materials are similar, corresponding to Dy 2 O 3 The (431) and (622) crystal planes of nanomaterials, Dy 2 O 3 The characteristic peak of the nanomaterial at 30° corresponding to the (222) crystal plane is annihilated, showing that the diffraction peak of the DUCN composite material at 27.5° is significantly wider than that of the UCN, confirming that a small amount of Dy was successfully doped into the UCN material. 2 O 3 However, no other impurity peaks were observed in the DUCN composite material, indicating that Dy 2 O 3 The doping did not affect the crystalline phase of the UCN material.

[0086] Then, the morphology of the prepared composites was studied visually using transmission electron microscopy (TEM). Figure 2 As shown in B. Figure 2 Ba can be seen to be different from the intrinsic morphology of graphite phase carbon nitride. The gC prepared by the present invention 3 N 4 It presents an ultra-thin morphology. In addition, a single Dy 2 O 3 It is composed of many particles about 20 nm in size gathered together ( Figure 2 Bb). Figure 2 Bc clearly shows that many Dy have become smaller 2 O 3 Evenly dispersed in ultra-thin gC 3 N 4 The high-resolution transmission electron microscopy image (omitted) also shows that the spacing is about 0.317 nm corresponding to Dy 2 O 3 The lattice fringes of the (222) crystal plane indicate that the ultrathin gC3 N 4 Successfully loaded Dy 2 O 3 Nanoparticles will help transfer charges during photoelectric conversion.

[0087] (2) The ultrathin gC in PBS (0.1 M pH = 7) buffer solution was studied in detail. 3 N 4 (UCN) modified electrode, Dy 2 O 3 Modified electrode, Dy prepared in Example 3 of the present invention 2 O 3 / Ultra-thin gC 3 N 4 The electrochemiluminescence (ECL) behavior of the composite (DUCN) modified electrode and the DUCN modified electrode after adding cysteine, such as Figure 3 As shown. It can be observed that a single Dy 2 O 3 There is almost no ECL signal when the modified electrode is used as a luminescent probe. In the absence of a luminophore, the electrochemiluminescence signal of a single UCN modified electrode is also extremely weak. However, after the two are combined and modified on a glassy carbon electrode, the ECL signal is significantly enhanced, indicating that Dy 2 O 3 The cathode electrochemiluminescence efficiency of UCN was strongly sensitized. Then, cysteine ​​was added. It was found that the ECL signal of the composite probe modified electrode was significantly weakened. Therefore, the addition of cysteine ​​was used to inhibit the immobilized Dy 2 O 3 / Ultra-thin gC 3 N 4 The ECL effect of the composite material modified electrode can establish a new system that responds to cysteine. Further research on the electrochemical signals of the single material and DUCN modified electrodes before and after the addition of cysteine ​​found that cysteine ​​only underwent an obvious oxidation reaction on the composite material modified electrode, confirming that the DUCN composite material increased the active sites and the loading rate of the target analyte cysteine, making it more reactive on the composite material modified electrode.

[0088] (3) Various assay conditions were optimized, including buffer medium, pH value, doping mass ratio, probe modifier deposition amount, etc. Under the optimal detection conditions, as the amount of cysteine ​​increased, Dy 2 O 3 / Ultra-thin gC 3 N 4 The ECL signal of the composite material modified electrode continued to decrease, indicating that cysteine ​​had a strong inhibitory effect on the ECL luminescence of the system, such as Figure 4As shown in Figure 2, the logarithm of the ECL intensity change value of the DUCN system and the natural logarithm of the cysteine ​​concentration are in the range of 0 ~ 1.0×10 -4 There is a good linear relationship in the range of mol / L, and the linear regression equation is lgΔ ECL =3.31ln C 半胱氨酸 (mol / L)+0.12(r=0.9950), according to the 3σ / S method (σ is the standard deviation of the blank solution, S is the slope of the linear equation), the detection limit is 0.27 μM. Compared with other existing ECL probes, this detection method has a wider linear detection range and a lower detection limit.

[0089] (4) To study Dy 2 O 3 / Ultra-thin gC 3 N 4 The specificity of the composite material modified electrode for cysteine ​​detection was investigated by adding several substances that may coexist with cysteine ​​into the system, including Cd 2+ , Cu 2+ , Pb 2+ , aminophylline, sodium cromoglycate, glucose, tyrosine, ribavirin, glycine, ascorbic acid and sarcosine were tested, such as Figure 5 The results show that the presence of other substances does not have a significant effect on the ECL signal of the DUCN system. Only the addition of cysteine ​​can significantly quench the ECL signal of the DUCN system, indicating that Dy 2 O 3 / Ultra-thin gC 3 N 4 The ECL sensor constructed with composite material probe has good recognition selectivity for cysteine. 2 O 3 / Ultra-thin gC 3 N 4 The composite modified electrode repeatedly measured the same concentration of cysteine ​​10 times, and the relative standard deviation was 2.74%, indicating that the composite modified electrode has good repeatability. In addition, after the prepared composite modified electrode was stored at room temperature for 3 days, the above cysteine ​​solution was measured again, and the ECL response only decreased by 5.1%, indicating that the composite probe has good long-term stability for detecting cysteine.

[0090] The above specific implementation method part specifically introduces the analytical method involved in the present invention. It should be noted that the above introduction is only to help those skilled in the art better understand the method and ideas of the present invention, rather than limiting the relevant content. Without departing from the principle of the present invention, those skilled in the art may also make appropriate adjustments or modifications to the present invention, and the above adjustments and modifications shall also fall within the scope of protection of the present invention.

Claims

1. A Dy 2 O 3 / Application of ultrathin graphene-phase carbon nitride composites in electrochemiluminescence sensing and quantitative detection of cysteine, It is characterized in that The Dy 2 O 3 The method for preparing the ultra-thin graphite phase carbon nitride composite material comprises the following steps: The first step is to use a certain amount of acetone to pre-treat urea for a certain period of time, remove the solvent, and then heat and calcine in a muffle furnace to obtain ultra-thin gC 3 N 4 ; The pretreatment time is 2-4 h, and the muffle furnace calcination parameters are: calcination at 450-650℃ for 3-6 h; Step 2: Add weighed Dy(NO 3 ) 3 •6H 2 O and ultrathin gC prepared by the first step reaction 3 N 4 , ultrasonic dispersion is used to form a uniform dispersion of the two in water, and then a certain temperature is set to stir the reaction; The third step is to centrifuge the material obtained in the previous step, wash it with ultrapure water, and then dry it in an oven; Step 4: Finally, the dried precursor is placed in a crucible, placed in a muffle furnace, and calcined at 450-650°C for 3-6 h at a heating rate of 5°C / min. After annealing, the target product Dy 2 O 3 / Ultra-thin gC 3 N 4 Composite materials.

2. The use according to claim 1, It is characterized in that In the first step, the dosage ratio of acetone to urea is 60-80 mL:8-15 g.

3. The use according to claim 1, It is characterized in that In the second step, ultrapure water and ultrathin gC 3 N 4 and Dy(NO 3 ) 3 •6H 2 The dosage ratio of O is 10-20 mL:200 mg:8-32 mg.

4. The use according to claim 1, It is characterized in that In the second step, the ultrasonic dispersion time is 8-15 min; the stirring reaction parameters are: temperature 65-75°C, time 4-8 h.

5. The use according to claim 1, It is characterized in that In the third step, oven drying parameters are as follows: drying at 70-90°C for 1-3 h.