A method for preparing non-stick cookware and the non-stick cookware obtained therefrom

By processing a composite material layer with a bionic lotus leaf structure on the inner surface of the pot substrate, the existing non-stick pots have been solved, and a longer service life and better non-stick effect are achieved.

CN116623118BActive Publication Date: 2024-11-15HANGZHOU ENTHALPY ZHIXING TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310631514.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-30
Publication Date
2024-11-15
Estimated Expiration
2043-05-30

AI Technical Summary

Technical Problem

The PTFE Teflon coating of existing non-stick pans is insufficient in temperature resistance, short service life and not resistant to dry burning. The pestle structure of the bionic lotus leaf non-stick pans is insufficient in hardness and cannot maintain long-lasting anti-stickness.

Method used

Process the composite material layer of a bionic lotus leaf structure on the inner surface of the pot substrate, including the first bonding phase, the second bonding phase and the high-carbon compound, and form holes and peak structures by heating, and perform high-energy fusing to form mastoids to form Structure, improve hardness and anti-stick effect.

Benefits of technology

It extends the service life of non-stick pans, improves resistance to high temperatures and scratches, enhances non-stick properties, avoids direct contact between food and pans, and ensures health and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116623118B_ABST
    Figure CN116623118B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a non-stick cookware and the non-stick cookware obtained, and relates to the field of cookware, comprising the following steps: S101, selecting a cookware matrix; S102, preparing a composite material, the composite material comprising a first bonding phase for increasing strength, a second bonding phase for assisting in increasing strength, and a high-carbon compound; S103, processing the composite material to the inner surface of the matrix to form a composite material layer; S104, heating the matrix to carbonize the high-carbon compound to form a plurality of cavities and spikes; S105, fusing the composite material layer to passivate the spikes to form a papilla structure. In the invention, the spikes formed by the composite metal layer are fusing-strengthened, thereby improving the strength of the composite metal layer and extending the service life of the prepared cookware.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cookware, and in particular to a method for preparing a non-stick cookware and the prepared non-stick cookware. Background Art

[0002] Currently, most non-stick cookware sold on the market is PTFE Teflon coated non-stick cookware. The maximum temperature resistance of the PTFE Teflon coating cannot exceed 250℃. After exceeding 250℃, its non-stick performance will rapidly decay and carbonize and fall off. Therefore, there are problems such as short coating life, poor resistance to dry burning and easy to fall off, which causes a large amount of metal material waste to the country every year. Even if the coating is not damaged, it will be slowly worn away by food and finally all eaten by the human body along with the dishes, which not only affects the service life of the product, but also endangers human health.

[0003] There are also bionic lotus leaf non-stick pans on the market, whose inner surface imitates the micro-nano structure of lotus leaf papillae, reducing the contact area between food and the bottom of the pan and establishing a physical non-stick barrier. The bionic lotus leaf non-stick pan papillae structure in the related art is not hard enough, and is not resistant to scratches by iron spatulas or high temperatures, and cannot maintain its non-stick properties for a long time. Summary of the invention

[0004] The present invention aims to solve one of the technical problems in the related art to a certain extent. To this end, the present invention provides a method for preparing a non-stick cookware, which has the advantage of long service life of the prepared non-stick cookware.

[0005] In order to achieve the above object, the present invention adopts the following technical solution:

[0006] A method for preparing a non-stick cookware comprises the following steps:

[0007] S101, selecting a cookware base;

[0008] S102, preparing a composite material, the composite material comprising a first bonding phase for increasing strength, a second bonding phase for assisting in increasing strength, and a high carbon compound;

[0009] S103, processing the composite material to the inner surface of the substrate to form a composite material layer;

[0010] S104, heating the substrate to carbonize the high carbon compound to form a plurality of cavities and peaks;

[0011] S105, fusing the composite material layer to blunt the peaks to form a papillary structure.

[0012] In the present invention, a composite material layer having a bionic lotus leaf structure is processed on the inner surface of the cookware base, and the bionic lotus leaf structure has a concave-convex morphology with a nipple structure. The composite material layer is in direct contact with the food, which reduces the contact area between the food and the cookware, so that the prepared cookware can achieve a non-stick cooking effect. It should be noted that the inner surface of the cookware base is defined as the side that should be in direct contact with the food, and the nipple structure is also formed on the side of the composite material layer that is in direct contact with the food, while the other side of the composite material layer is in contact with the inner surface of the cookware.

[0013] The composite material includes a first bonding phase, a second bonding phase and a high carbon compound, and the composite material is processed to the inner surface of the matrix to form a composite material layer. The composite material contains a high carbon compound. When the inner surface of the matrix is ​​heated, the high carbon compound will carbonize and become brittle, thereby forming a cavity structure with low surface energy. The inner surface of the composite material layer (i.e., the side in direct contact with the food) is of course also distributed with the cavity structure. The inner surface of the composite material layer presents an uneven micro-topography with cavities and peaks, which reduces the contact area between the food and the pot and prevents sticking to the pot. In addition, the cavity structure can absorb air and store grease. During the heating process, hot air and oil mist will be generated, which can hold up the food. At the same time, the cavity structure will reduce the contact area between the food and the pot, thereby playing a physical non-stick role.

[0014] The inner surface of the composite material layer is melted and the peaks are passivated to form dense arc-shaped particles, namely the papillary structure, whose surface free energy is reduced. After melting, the hardness of the peaks is increased, making the composite material layer more resistant to scratches by spatulas and extending the service life of the cookware.

[0015] Optionally, the composite material layer is melted by plasma or laser to passivate the peaks, and the hardness of the mastoid structure formed after melting is 800-1200HV. The inner surface of the composite material layer is melted by a high energy density plasma beam or laser beam, and the peaks on the inner surface are passivated to form a mastoid structure, which reduces the surface energy of the inner surface and improves the non-stick effect. The hardness of the mastoid structure formed after high-energy melting is increased to 800-1200HV.

[0016] Optionally, in step S102, the carbonization temperature of the selected high carbon compound is lower than 600° C. In the present invention, it is necessary to add a high carbon compound to the composite material so that the high carbon compound can be subsequently carbonized and form cavities in the composite material layer. Selecting a high carbon compound with a lower carbonization temperature can form cavities in the composite material layer at a relatively low temperature, which is beneficial to improving efficiency and saving energy.

[0017] Optionally, in step S104, the inner surface of the substrate is heated and carbonized for 0.5 to 1 hour. The substrate is maintained at a temperature above the carbonization temperature of the high carbon compound for 0.5 to 1 hour to form a cavity structure with low surface energy.

[0018] Optionally, the composite material includes the following components in mass percentage: 40% to 70% of the first bonding phase, 15% to 50% of the second bonding phase, and 5% to 10% of the high carbon compound. The first bonding phase accounts for the largest proportion of the mass of the composite material, and is used to enhance the hardness and bond other substances in the composite material, and is also used to bond the composite material to the cookware substrate. The second bonding phase is used to assist the bonding of the first bonding phase, further strengthen the bonding between the materials, and also make the connection between the composite material layer and the substrate more firmly. The high carbon compound is used to heat the substrate and carbonize it to form holes and spikes.

[0019] Optionally, the first bonding phase is one or more of titanium, titanium alloy, zirconium, zirconium alloy, molybdenum, molybdenum alloy, hafnium, hafnium alloy and stainless steel. The first bonding phase is a metal with high hardness and high strength, which provides a certain strength for the composite material layer, making the composite material layer more wear-resistant and easy to clean even under high temperature or high-intensity scraping. The composite material layer is not easy to fall off when the pot is heated or cooked at high temperature.

[0020] Optionally, the second bonding phase is one or more of silicate, diatomaceous earth, silicon oxide and titanium oxide. The second bonding phase can help enhance the hardness of the composite material layer and improve the scratch resistance. Silicate and diatomaceous earth have low melting points and can form a porous structure at a high temperature above the melting point, which is conducive to grease penetration.

[0021] Optionally, the high carbon compound is one or more of acrylic resin, stearic acid, fatty acid, starch, and fiber. The carbonization temperature of acrylic resin is 200-300° C., while stearic acid will decompose above 200° C. After the acrylic resin or stearic acid is carbonized, the composite material layer forms a multi-hole structure.

[0022] Optionally, in step S102, when preparing the composite material, the first binder phase, the second binder phase and the high carbon compound are dispersed, ground and mixed uniformly, and then granulated into particles with a particle size of 100 to 450 mesh. The first binder phase, the second binder phase and the high carbon compound are placed in a dispersion grinder for dispersion grinding, and the three are mixed uniformly, so that the holes formed after the subsequent carbonization of the high carbon compound are evenly distributed in the composite material layer. The composite material after dispersion grinding is formed into particles with a particle size of 100 to 450 mesh by a granulator.

[0023] Optionally, in step S103, the particles of the composite material with a particle size of 100 to 450 mesh are processed to the inner surface of the substrate by thermal spraying, plasma spraying, cold spraying or laser cladding to form a composite metal layer. It should be noted that the composite material obtained by dispersing and grinding the first binder phase, the second binder phase and the high carbon compound and mixing them uniformly is suitable for being processed to the inner surface of the substrate by thermal spraying, plasma spraying, cold spraying or laser cladding.

[0024] Optionally, in step S102, when preparing the composite material, the first binder phase, the second binder phase and the high carbon compound are configured as a core-encapsulated structure; wherein the first binder phase forms an outer skin, and the second binder phase and the high carbon compound are dispersed, ground and granulated and then filled into the outer skin. Only the second binder phase and the high carbon compound are dispersed, ground and granulated, and then filled into the outer skin formed by the first binder phase to form a core-encapsulated structure.

[0025] Optionally, in step S103, the composite material prepared in step S102 is processed onto the inner surface of the substrate by arc spraying, laser spraying or plasma cladding. It should be noted that when the composite material is processed onto the inner surface of the substrate by arc spraying, laser spraying or plasma cladding, the composite material does not maintain a core-wrapped structure, but is atomized and broken up to form a relatively uniform state, so that holes can be formed on the inner surface of the composite material layer.

[0026] Optionally, after step S105, there is a step S106, in which vegetable oil and / or silicone oil is applied to the inner surface of the substrate to allow the vegetable oil and / or silicone oil to penetrate into the cavities, modify the composite material layer on the inner surface of the substrate, and improve the initial non-stick effect of the cookware. Specifically, immersion, spraying, wiping, etc. are used to allow the grease to penetrate into the cavities.

[0027] In addition, the present invention also provides a non-stick cookware, which is prepared by any of the above-mentioned preparation methods. The reasoning process of the beneficial effects of the non-stick cookware provided by the present invention and the above-mentioned preparation method is similar, and will not be repeated here.

[0028] 1. In the present invention, a composite material layer with a bionic lotus leaf structure is processed on the inner surface of the cookware base to achieve the purpose of anti-sticking. The bionic lotus leaf structure includes a number of cavities that can absorb air and store grease. During the heating process, hot air and oil mist will be generated to hold up the food. At the same time, the cavity structure will reduce the contact area between the food and the cookware, thereby achieving a physical non-stick effect.

[0029] 2. The composite material contains high carbon compounds, which are carbonized at high temperatures to form adjacent cavities and peaks in the composite material layer. After the peaks are melted at high energy, they are passivated to form a papillary structure. The surface energy of the papillary structure is lower than that of the peak structure, which further improves the anti-sticking ability; and the hardness of the papillary structure formed after melting increases, which improves the anti-scratch ability and extends the service life of the cookware.

[0030] 3. The composite material includes a first bonding phase composed of a high-hardness metal and a second bonding phase composed of a ceramic material such as silicate, which improves the hardness of the composite material layer and enhances the anti-scratch ability.

[0031] These features and advantages of the present invention will be disclosed in detail in the following specific embodiments and drawings. The best embodiments or means of the present invention will be described in detail in conjunction with the drawings, but they are not intended to limit the technical solutions of the present invention. In addition, there are multiple features, elements, and components that appear in each of the following texts and drawings, and different symbols or numbers are marked for convenience, but they all represent components with the same or similar structures or functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The present invention will be further described below in conjunction with the accompanying drawings:

[0033] Figure 1 Schematic diagram of the microstructure of the composite material prepared in Example 1 of the present invention;

[0034] Figure 2 Schematic diagram of the microstructure of the composite material prepared in Example 2 of the present invention;

[0035] Figure 3 It is a schematic diagram of the structure of the spike when the composite material layer is not melted;

[0036] Figure 4 Schematic diagram of the structure of the papillary structure generated after the composite material layer is melted.

[0037] Among them, 1. the first bonding phase; 2. the second bonding phase; 3. high carbon compounds. DETAILED DESCRIPTION

[0038] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.

[0039] References in this specification to "one embodiment" or "an example" or "an example" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment of the present patent disclosure. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.

[0040] Embodiment 1:

[0041] This embodiment provides a method for preparing a non-stick cookware, comprising the following steps:

[0042] S101, selecting a cookware base; cleaning the base to remove oxides and contaminants on the surface thereof.

[0043] S102, preparing a composite material, the composite material comprising a first bonding phase 1, a second bonding phase 2 and a high carbon compound 3; weighing the raw materials according to the following mass percentages: 70% for the first bonding phase 1, 25% for the second bonding phase 2, and 5% for the high carbon compound 3. In this embodiment, the first bonding phase 1 is a titanium alloy, the second bonding phase 2 is a silicate, and the high carbon compound 3 is an acrylic resin. In other embodiments, the first bonding phase 1 may also be one or more of zirconium, zirconium alloy, molybdenum, molybdenum alloy, hafnium, hafnium alloy and stainless steel; the second bonding phase 2 may also be a ceramic material such as diatomaceous earth; and the third bonding phase may also be stearic acid.

[0044] The first bonding phase 1 is selected as the outer skin, and the second bonding phase 2 and the high carbon compound 3 are prepared into a wire material with a diameter of 1.2 to 2.2 mm. The first bonding phase 1, the second bonding phase 2 and the high carbon compound 3 are formed as follows Figure 1 The core structure shown.

[0045] S103, processing the composite material to the inner surface of the substrate to form a composite material layer; specifically, using arc spraying equipment to spray the composite material to the inner surface of the substrate. The arc spraying equipment has an operating voltage of 25-40V, an operating current of 70-200A, and an air pressure of 1.0-1.5Mpa. The thickness of the composite material layer finally generated is 0.02-0.06mm, and the hardness is 400-600HV.

[0046] S104, heating the substrate to carbonize the high carbon compound 3 to form a plurality of cavities and peaks; specifically, placing the substrate in a high temperature furnace and baking it at 450° C. for 0.5 h to carbonize the acrylic resin, and forming peaks and cavities in the composite material layer.

[0047] S105, melting the composite material layer to passivate the peaks to form a papillary structure; specifically, using a high-power laser of 5 to 20 kW, focusing on the peaks on the inner surface of the composite material layer, melting the peaks at a speed of 5 to 10 cm / s to form a smooth and dense papillary structure, the hardness of the papillary structure is 800 to 1200 HV, thereby improving the strength of the composite material layer.

[0048] This embodiment also provides a non-stick cookware, which is made by the above steps and is subjected to a non-stick test and a long-lasting non-stick test. The test results are shown in Table 1.

[0049] Example 2

[0050] This embodiment provides a method for preparing a non-stick cookware, which is different from the embodiment 1 mainly in that the method for preparing the composite material is different, and the method comprises the following steps:

[0051] S101, selecting a cookware base; cleaning the base to remove oxides and contaminants on the surface thereof.

[0052] S102, preparing a composite material, the composite material comprising a first bonding phase 1, a second bonding phase 2 and a high carbon compound 3; weighing the raw materials according to the following mass percentages: 70% for the first bonding phase 1, 25% for the second bonding phase 2, and 5% for the high carbon compound 3. In this embodiment, the first bonding phase 1 is a titanium alloy, the second bonding phase 2 is a silicate, and the high carbon compound 3 is an acrylic resin. In other embodiments, the first bonding phase 1 may also be one or more of zirconium, zirconium alloy, molybdenum, molybdenum alloy, hafnium, hafnium alloy and stainless steel; the second bonding phase 2 may also be a ceramic material such as diatomaceous earth; and the third bonding phase may also be stearic acid.

[0053] The first binder phase 1, the second binder phase 2 and the high carbon compound 3 are placed in a dispersion grinder for dispersion grinding and the three are mixed evenly so that the holes formed after the subsequent carbonization of the high carbon compound 3 are evenly distributed in the composite material layer. The composite material after dispersion grinding is formed by a granulator as follows Figure 2 The particle sizes shown are 100-450 mesh particles.

[0054] S103, processing the composite material to the inner surface of the substrate to form a composite material layer; specifically, using a thermal spraying device to spray the composite material to the inner surface of the substrate. The thickness of the composite material layer finally generated is 0.02 to 0.06 mm, and the hardness is 400 to 600 HV. In other embodiments, the composite material can also be processed to the inner surface of the substrate by plasma spraying or laser cladding.

[0055] S104, heating the substrate to carbonize the high carbon compound 3 to form a plurality of cavities and peaks; specifically, placing the substrate in a high temperature furnace and baking it at 450° C. for 0.5 h to carbonize the acrylic resin, and forming peaks and cavities in the composite material layer.

[0056] S105, melting the composite material layer to passivate the peaks to form a papillary structure; specifically, using a high-power laser of 5 to 20 kW, focusing on the peaks on the inner surface of the composite material layer, melting the peaks at a speed of 5 to 10 cm / s to form a smooth and dense papillary structure, the hardness of the papillary structure is 800 to 1200 HV, thereby improving the strength of the composite material layer.

[0057] This embodiment also provides a non-stick cookware, which is made by the above steps and is subjected to a non-stick test and a long-lasting non-stick test. The test results are shown in Table 1.

[0058] Comparative Example

[0059] This comparative example provides a method for preparing a non-stick cookware, which is different from Example 1 mainly in that the composite material layer is not subjected to high-energy melting. The method comprises the following steps:

[0060] S101, selecting a cookware base; cleaning the base to remove oxides and contaminants on the surface thereof.

[0061] S102, preparing a composite material, the composite material comprising a first bonding phase 1, a second bonding phase 2 and a high carbon compound 3; weighing the raw materials according to the following mass percentages: 70% for the first bonding phase 1, 25% for the second bonding phase 2, and 5% for the high carbon compound 3. In this embodiment, the first bonding phase 1 is a titanium alloy, the second bonding phase 2 is a silicate, and the high carbon compound 3 is an acrylic resin. In other embodiments, the first bonding phase 1 may also be one or more of zirconium, zirconium alloy, molybdenum, molybdenum alloy, hafnium, hafnium alloy and stainless steel; the second bonding phase 2 may also be a ceramic material such as diatomaceous earth; and the third bonding phase may also be stearic acid.

[0062] The first binder phase 1, the second binder phase 2 and the high carbon compound 3 are placed in a dispersion grinder for dispersion grinding, and the three are mixed evenly, so that the holes formed after the subsequent carbonization of the high carbon compound 3 are evenly distributed in the composite material layer. The composite material after dispersion grinding is made into particles with a particle size of 100 to 450 meshes by a granulator.

[0063] S103, processing the composite material to the inner surface of the substrate to form a composite material layer; specifically, using a thermal spraying device to spray the composite material to the inner surface of the substrate. The thickness of the composite material layer finally generated is 0.02 to 0.06 mm, and the hardness is 400 to 600 HV. In other embodiments, the composite material can also be processed to the inner surface of the substrate by plasma spraying or laser cladding.

[0064] S104, heating the substrate to carbonize the high carbon compound 3 to form a plurality of cavities and peaks; specifically, placing the substrate in a high temperature furnace and baking it at 450° C. for 0.5 h to carbonize the acrylic resin, and forming peaks and cavities in the composite material layer.

[0065] This comparative example also provides a non-stick cookware, which is made by the above steps and is subjected to a non-stick test and a long-lasting non-stick test. The test results are shown in Table 1.

[0066] The specific test methods for non-stick test and long-lasting non-stick test are as follows:

[0067] Non-stick test: The test is carried out in accordance with the requirements of GB32095.1-2015 and is divided into levels I, II and III. Level I has the best non-stickiness and level III has the worst non-stickiness.

[0068] Long-lasting non-stick test: Test in accordance with GB32388-2015 requirements. The unit is the number of times. The higher the number, the longer the life. The non-stick result is evaluated every 1,000 times, and the number of times when it is used to level III is recorded.

[0069] Table 1: Non-stickiness and long-lasting non-stickiness test results of Example 1, Example 2 and Comparative Example

[0070] serial number Non-stick Long-lasting non-stickiness (times) Embodiment 1 I 15000 Embodiment 2 I 14000 Comparative Example II 8000

[0071] As can be seen from Table 1, the non-stick properties of Example 1 and Example 2 after high-energy melting are better than those of the comparative example, and the service life is also better than that of the comparative example.

[0072] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

Claims

1. A method for preparing a non-stick cookware, characterized in that: The steps include: S101, selecting a cookware base; S102, preparing a composite material, the composite material comprising a first binder phase (1) for increasing strength, a second binder phase (2) for assisting in increasing strength, and a high carbon compound (3); when preparing the composite material, the first binder phase (1), the second binder phase (2), and the high carbon compound (3) are configured into a core-wrapped structure; wherein the first binder phase (1) forms an outer skin, and the second binder phase (2) and the high carbon compound (3) are dispersed, ground, and granulated before being filled into the outer skin; The first binder phase (1) is one or more selected from the group consisting of titanium, titanium alloy, zirconium, zirconium alloy, molybdenum, molybdenum alloy, hafnium, hafnium alloy and stainless steel; the second binder phase (2) is one or more selected from the group consisting of silicate, diatomaceous earth, silicon oxide and titanium oxide; the high carbon compound (3) is one or more selected from the group consisting of acrylic resin, fatty acid, starch and fiber; S103, processing the composite material to the inner surface of the substrate to form a composite material layer; S104, heating the substrate to carbonize the high carbon compound (3) to form a plurality of cavities and peaks; S105, fusing the composite material layer to blunt the peaks to form a papillary structure.

2. The preparation method according to claim 1, characterized in that: In step S105, the composite material layer is melted by plasma or laser to passivate the peaks, and the hardness of the papillary structure formed after melting is 800-1200 HV.

3. The preparation method according to claim 1, characterized in that: In step S102, the carbonization temperature of the selected high carbon compound (3) is lower than 600°C.

4. The preparation method according to claim 1, characterized in that: In step S104, the inner surface of the substrate is heated and carbonized for 0.5 to 1 hour.

5. The preparation method according to any one of claims 1 to 4, characterized in that The composite material comprises the following components in percentage by mass: 40% to 70% of a first bonding phase (1), 15% to 50% of a second bonding phase (2), and 5% to 10% of a high carbon compound (3).

6. The preparation method according to claim 1, characterized in that: In step S103, the composite material is processed onto the inner surface of the substrate by arc spraying, laser spraying or plasma cladding.

7. The preparation method according to claim 1, characterized in that: After step S105, there is step S106, in which vegetable oil and / or silicone oil is applied to the inner surface of the substrate to allow the vegetable oil and / or silicone oil to penetrate into the cavities.

8. A non-stick cookware, characterized in that: Prepared by the preparation method according to any one of claims 1 to 7.