A method for preparing a special-shaped semiconductor target

Through the process flow of forging, rolling, annealing and secondary forging, the problems of high cost and poor structural uniformity in the preparation of semiconductor special-shaped targets are solved, and low-cost and efficient preparation of targets with good uniformity is achieved, which meets the requirements of high purity and Dimensional precision requirements.

CN116791044BActive Publication Date: 2024-10-22GEMCH MATERIAL TECH SUZHOU
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211580108.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-22
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The existing preparation process of semiconductor special-shaped targets has problems such as high cost and poor internal structure uniformity, resulting in large losses and difficulty in meeting the needs of high purity and dimensional precision.

Method used

Adopting the process flow of raw materials - forging - rolling - annealing - secondary forging - machining, the grains are broken through forging and rolling, and the annealing and secondary forging homogenize the material, reducing losses and costs.

Benefits of technology

It achieves low-cost and efficient preparation of special-shaped semiconductor targets with good uniformity, reduces the original drilling process of thick blanks, reduces manufacturing costs, and improves the uniformity of the internal structure of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116791044B_ABST
    Figure CN116791044B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a special-shaped semiconductor target, relates to the field of semiconductor target preparation, and aims to solve the problems of high preparation cost and poor internal structural uniformity of the current special-shaped semiconductor target. The main points of the technical solution are: 1) raw material preparation; 2) mold and equipment preparation; 3) raw material preheating; 4) forging; 5) rolling: cold rolling or hot rolling is selected according to different raw material materials; 6) annealing: different annealing temperatures and holding times are set according to different raw material materials; 7) secondary forging: different mold sizes are designed according to the finished product size, and the raw materials are preheated and placed on the forging mold for forging; 8) machining: the forged special-shaped blank is directly machined to obtain the finished product. The method for preparing a special-shaped semiconductor target of the invention has low cost and good internal structural uniformity of the target.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of semiconductor target material preparation, and more specifically, to a method for preparing a special-shaped semiconductor target material. Background Art

[0002] Target materials are also called "sputtering targets" because they are the target materials bombarded by high-speed metal plasma flow during the sputtering process. Target materials are the core raw materials for preparing functional thin films in the fields of semiconductors, display panels, photovoltaics, etc., and they are irreplaceable in the process. Replacing different target materials can obtain different film systems, thereby achieving functions such as conductivity or blocking.

[0003] In general, the purity, density, composition uniformity, and grain size of the target material will have a certain impact on the coating performance, and the degree and focus of the impact will vary for different downstream products.

[0004] Among various types of target materials, semiconductor targets have the highest technical requirements, and their purity requirements are usually as high as 5N5 or above; and there are also extremely high requirements for dimensional precision.

[0005] The main types of metal sputtering targets used in the semiconductor chip industry include: high-purity sputtering targets such as aluminum, copper, titanium, tantalum, cobalt and tungsten, as well as sputtering targets of alloys such as aluminum-silicon-copper.

[0006] For semiconductor special-shaped targets, the current main process is: raw materials - forging - hollowing - machining. This method has high losses, high costs, and poor internal structural uniformity. A process method that reduces costs and improves internal structure is needed.

[0007] Therefore, a new solution needs to be proposed to solve this problem. Summary of the invention

[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing a special-shaped semiconductor target material, which processes the target material by the method of raw material - forging - rolling - annealing - secondary forging - machining, which not only has low cost but also can ensure the uniformity of the internal structure and small loss.

[0009] The above technical objectives of the present invention are achieved through the following technical solutions: A method for preparing a special-shaped semiconductor target, characterized in that it comprises the following steps:

[0010] 1) Raw material preparation: Calculate the deformation amount according to the required size of the finished product and the internal structure requirements, so as to calculate the required raw material ingot size and prepare the raw materials;

[0011] 2) Preparation of molds and equipment: According to different materials and different size requirements, choose forging and rolling machines of different tonnages, and design different mold shapes and sizes according to the shape and size of the finished product;

[0012] 3) Preheating of raw materials;

[0013] 4) Forging: Calculate the forging ratio and select a suitable forging machine for forging according to product material, finished product size and finished product grain requirements;

[0014] 5) Rolling: Choose cold rolling or hot rolling according to the raw material;

[0015] 6) Annealing: Set different annealing temperatures and holding times according to the material of the raw materials;

[0016] 7) Secondary forging: Design different die sizes according to the finished product size, preheat the raw materials and place them on the forging die for forging;

[0017] 8) Machining: The forged special-shaped blank is directly machined to obtain the finished product.

[0018] By adopting the above technical solution,

[0019] The present invention is further configured as follows: in step 1, the raw material is high-purity aluminum or copper or titanium or tantalum metal or aluminum-silicon-copper alloy material, with a purity of ≥99.9995%.

[0020] The present invention is further configured as follows: in step 4, the forging speed is 5.25-20 mm / s, the pressure is maintained for 1 minute each time, and the forging is continued for 5-10 times, so that the cylindrical ingot of the raw material is forged into a round cake until the desired size is reached.

[0021] The present invention is further configured as follows: in step 4, the pressing amount for each pass is set according to the hardness of the raw material and the number of rolling passes is set according to the starting thickness and the target thickness, the pressing amount for each pass is 0.5 mm to 15 mm, and the maximum pressing amount is selected within the range of equipment capacity and material deformation capacity.

[0022] The present invention is further configured as follows: in step 7, the upper and lower dies are squeezed mutually during forging, so that the raw material is forged from a round cake shape into a target irregular-shaped blank.

[0023] The present invention is further configured as follows: in step 3, the shortest heating time is maintained under the condition that the blank is evenly heated through.

[0024] The present invention is further configured as follows: in step 3, under the premise that overheating does not occur, the initial forging temperature is increased and the heating times are reduced.

[0025] The present invention is further configured as follows: in step 4 and step 7, the initial forging temperature is 100 to 200 degrees below the melting point of the raw material.

[0026] The present invention is further configured as follows: in step 4 and step 7, the final forging temperature at the end of forging is higher than the recrystallization temperature of the raw material.

[0027] In summary, the present invention has the following beneficial effects: through the process steps of raw material - forging - rolling - annealing - secondary forging - machining, the raw material blank is processed into the required special-shaped target material, especially by forging, rolling and annealing and then performing secondary forging again, which reduces the process of boring holes in the original thick blank, reduces losses, and is beneficial to material uniformity, thereby obtaining a target material with uniform internal structure and reducing manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 It is a schematic diagram of the processing flow of the present invention;

[0029] Figure 2 This is the metallographic detection diagram of Example 1. DETAILED DESCRIPTION

[0030] The present invention is described in detail below in conjunction with the accompanying drawings and embodiments.

[0031] The present invention adopts a novel method for preparing a special-shaped semiconductor high-purity metal or alloy target. The main process is as follows: Figure 1 The process includes raw material preparation - metal forging - metal rolling - metal annealing - metal secondary forging - machining.

[0032] This method is not limited to materials, including but not limited to high-purity metals such as aluminum, copper, titanium, tantalum, or alloy materials such as aluminum-silicon-copper.

[0033] The preparation protocol includes the following steps:

[0034] 1) Raw material preparation: In the early stage, the deformation is calculated according to the required size of the finished product and the internal structure requirements, so as to calculate the required raw material ingot size, prepare high-purity aluminum, copper, titanium, tantalum and other metal raw materials and aluminum-silicon-copper alloy materials, basically cylindrical raw material embryos, with a purity of up to 99.9995%;

[0035] 2) Preparation of molds and equipment: According to different materials and different size requirements, choose forging and rolling machines of different tonnages, and design different mold shapes and sizes according to the shape and size of the finished product;

[0036] 3) Preheating of raw ingots: The purpose of billet heating is to improve the plasticity of the billet and reduce the deformation resistance. Under the condition that the billet is evenly heated, the heating time should be shortened as much as possible to reduce defects such as metal oxidation and reduce fuel consumption. Forging should be carried out within a certain temperature range. The forging temperature is divided into the starting forging temperature and the ending forging temperature: the starting forging temperature is 100 to 200 degrees below the melting point of the material, and the final forging temperature refers to the sufficient plasticity at this time. Under the premise of not overheating, the starting forging temperature should be increased as much as possible to make the billet have the best forging performance, reduce the number of heating times, and improve productivity. The final forging temperature needs to be higher than the recrystallization temperature of the metal to ensure sufficient plasticity and to obtain a recrystallized structure after forging. If the final forging temperature is too high, coarse grains are easily formed and the mechanical properties are reduced; if the final forging temperature is too low, the forging performance will deteriorate.

[0037] 4) Metal forging: The metal forging process can break the internal grains of the metal longitudinally, thereby achieving a fine grain effect. Calculate the optimal forging ratio and select a suitable forging machine, such as 1000T, 2500T, 5000T, etc., based on the product material, finished product size and finished product grain requirements; similarly, select the optimal heating temperature and holding time based on the product material and forging ratio, then place the heated and held raw material embryo on the forging machine die, start the forging machine, set the forging speed to 5.25-20mm / s, hold the pressure for 1min each time, and continue forging for 5-10 times, so that the raw material embryo cylindrical ingot is forged into a round cake until it reaches the required size;

[0038] 5) Metal rolling: The metal rolling process can cause the internal grains of the metal to break laterally again. Depending on the metal material, cold rolling or hot rolling can be selected. For example, metal aluminum and aluminum alloys, metal titanium can be cold rolled, while metal copper and metal tantalum can be hot rolled. Set the amount of pressure for each pass according to the hardness of the material, and set the number of rolling passes according to the starting thickness and target thickness. The amount of pressure for each pass can be 0.5mm to 15mm. Select the maximum amount of pressure within the equipment capacity and material deformation capacity to destroy the grains to the greatest extent, thereby achieving a fine grain effect. Try to ensure that the material is flat and not warped during the rolling process, otherwise it needs to be leveled;

[0039] 6) Metal annealing: The metal annealing process is a process of grain homogenization, which can improve the uniformity of target product performance. Different annealing temperatures and holding times are set according to different metal materials. For example, for metal Al and Al alloys, the annealing temperature is set at 400℃~500℃ and the holding time is 1h~3h;

[0040] 7) Secondary metal forging: Secondary metal forging is a key step for special-shaped parts. This step is conducive to forming the final target product machining blank, which reduces the process of punching holes in the original thick blank, helps reduce losses, and is conducive to material uniformity. Different die sizes are designed according to the size of the finished product. Similar to the first forging process, the raw ingot is preheated and placed on the forging die. The forging machine is started, and the mutual extrusion of the upper and lower dies is used to forge the material from a round cake into a target special-shaped blank. Most of these special shapes are concave and convex.

[0041] 8) Metal machining: Forged special-shaped blanks can be directly machined to obtain finished products. Different blades can be selected according to different materials to avoid sticking. After processing, the products can undergo subsequent surface treatment, cleaning and other processes.

[0042] Embodiment 1:

[0043] The following is a specific description using AlSi alloy ingot as raw material:

[0044] 1) Raw material preparation: Use AlSi alloy ingots with a purity of 99.9995%, Si accounts for 3%, and the raw material ingot size is

[0045] 2) Equipment and mold selection: According to the soft properties of AlSi material, select 2500T press, and design the mold according to the finished product size: the primary forging mold is: upper mold 400*400*50mm, lower mold outer ring 400*400*50mm, inner ring is: The secondary forging die is: the upper die is convex, the lower die is concave, and the diameter of the upper die convex outlet is The protruding thickness is 26mm; the diameter of the lower die recess is The depth of the depression is 24mm;

[0046] 3) Preheating of raw ingots: According to the AlSi material and the size of the raw ingots, the preheating temperature is designed to be 500°C, and the temperature is kept for 1.5 hours to improve plasticity, increase deformation resistance and minimize metal oxidation;

[0047] 4) Metal forging: Use a 2500T forging press to place the preheated raw material embryo in the middle of the lower die of the primary forging die, start the forging press, set the forging speed to 15mm / s, hold the pressure for 1min each time, and continue forging for 5 times, so that the raw material embryo cylindrical ingot is forged into a round cake until it reaches the required size. The forging ratio is 3.6, which can achieve the effect of longitudinal crushing of internal grains;

[0048] 5) Metal rolling: Place the round cake with residual heat on the rolling mill for rolling, which can break the internal grains horizontally and refine the grains. The thickness before rolling is 30mm, the thickness after rolling is 15mm, the deformation is 50%, and the number of rolling passes is designed to be 6 times, with a downward pressure of 2-5mm per pass. After each rolling pass, rotate 90° before the next pass; after rolling, check the warpage. If the warpage is greater than 0.2mm, it needs to be leveled until it meets the requirements; the size after rolling is

[0049] 6) Metal annealing: For AlSi alloy, the annealing temperature is set to 450°C and the holding time is 2.5h. This is the process of homogenizing the grains, thereby improving the uniformity of the target product performance;

[0050] 7) Secondary forging of metal: Place the annealed sheet on the secondary forging die of the forging press, start the forging press, set the forging speed to 20 mm / s, and keep the pressure for 1 min each time, and continue forging for 6 times to finally form a special-shaped blank, which is convenient for subsequent processing, reduces material loss, and is conducive to material uniformity;

[0051] 8) Metal machining: According to the drawings, the AlSi blank of the special-shaped part is directly processed into the finished product. The finished product can undergo subsequent surface treatment, cleaning and other processes.

[0052] The AlSi alloy target obtained was observed, and the metallographic image obtained is shown in the attached figure. Figure 2 As shown, its internal structure is uniform and its grain grade reaches level 5, which fully meets customer needs.

[0053] The above is only a preferred embodiment of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a special-shaped semiconductor target, characterized in that: The following steps are involved: 1) Raw material preparation: Calculate the deformation amount according to the required size of the finished product and the internal structure requirements, so as to calculate the required raw material ingot size and prepare the raw materials; 2) Mold and equipment preparation: Select forging and rolling machines of different tonnages according to different materials and different size requirements, and design different mold shapes and sizes according to the shape and size of the finished product; 3) Preheating of raw materials; 4) Forging: Calculate the forging ratio and select a suitable forging machine for forging according to product material, finished product size and finished product grain requirements; 5) Rolling: Choose cold rolling or hot rolling according to the raw material; 6) Annealing: Set different annealing temperatures and holding times according to the different raw materials; 7) Secondary forging: Design different die sizes according to the finished product size, preheat the raw material and place it on the forging die for forging. During forging, the upper and lower dies are squeezed against each other to forge the raw material from a round cake into a target irregular-shaped blank; 8) Machining: The forged special-shaped blank is directly machined to obtain the finished product.

2. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In step 1, the raw material is high-purity aluminum or copper or titanium or tantalum metal or aluminum-silicon-copper alloy material with a purity of ≥99.9995%.

3. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In step 4, the forging speed is 5.25-20 mm / s, the pressure is maintained for 1 minute each time, and the forging is continued for 5-10 times, so that the cylindrical ingot of the raw material is forged into a round cake until the desired size is reached.

4. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In step 4, the pressing amount for each pass is set according to the hardness of the raw material, and the number of rolling passes is set according to the starting thickness and the target thickness. The pressing amount for each pass is 0.5 mm to 15 mm. The maximum pressing amount is selected within the range of equipment capacity and material deformation capacity.

5. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In step 3, the shortest heating time is maintained under the condition that the blank is evenly heated through.

6. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In step 3, without causing overheating, increase the initial forging temperature and reduce the number of heating times.

7. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In steps 4 and 7, the initial forging temperature is 100 to 200 degrees below the melting point of the raw materials.

8. The method for preparing a special-shaped semiconductor target according to claim 1, characterized in that: In step 4 and step 7, the final forging temperature at the end of forging is higher than the temperature at which the raw material recrystallizes.