Silicon modified high temperature high strength zirconia continuous fiber and its preparation method and application
By introducing a silicon source into the continuous zirconia fiber, a silicon-modified structure is formed to inhibit grain growth, and the problem of degradation of mechanical properties of zirconia fibers at high temperatures is solved, and high-strength and high-temperature stable fiber performance is achieved. It is suitable for Various high temperature applications.
Patent Information
- Application Number
- CN202311046103.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-08-18
AI Technical Summary
The grain size of existing zirconia continuous fibers increases at high temperatures, resulting in a decrease in mechanical properties, which cannot effectively inhibit grain growth, limiting its application range and service time.
By introducing a silicon source into the organozirconium source precursor, the ratio of the silicon source to the zirconium source is controlled to form silicon modified zirconium oxide continuous fibers, inhibit the growth of zirconium oxide grains, and prevent the precipitation of silicon, forming amorphous silicon oxide and tetragonal quadrilateral. Or the biphasic structure of cubic phase zirconia increases grain boundary diffusion barrier, reduces pore defects, and delays grain enclosure.
Under high temperature conditions of 1300℃~1500℃, the tensile strength of silicon modified zirconia continuous fiber reaches 2.0GPa~3.0GPa, the radius of curvature is 0.4mm~1mm, maintaining good mechanical properties, and reducing grain size by 50%. It is suitable for High temperature structure reinforcement, refractory and heat insulation materials.
Smart Images

Figure CN116815355B_ABST
Abstract
Description
Technical field:
[0001] The invention relates to a high-temperature and high-strength silicon-modified zirconia continuous fiber and a preparation method and application thereof, belonging to the field of inorganic non-metallic materials. Background technology:
[0002] High temperature resistant fiber is an important component of ceramic matrix composites, which solves the problems of low fracture toughness, low reliability and poor thermal shock resistance of ceramic matrix composites. Continuous ceramic fiber has the characteristics of high toughness, high specific modulus, high strength and weavability, so that the fiber reinforcement formed by it has excellent designability in terms of fiber components, weaving molding methods and gradient, and meets the requirements of prototype and temperature resistance under extreme conditions. Among the continuous oxide fibers, zirconium oxide fiber has outstanding advantages such as high melting point, high hardness, good chemical stability, high mechanical properties, the lowest thermal conductivity and the lowest saturated vapor pressure among oxides, which ensures that ZrO2 crystal fiber can maintain stable performance under extreme conditions. However, after long-term high temperature treatment, the grain size of ZrO2 crystal fiber increases and the fiber strength decreases significantly, which greatly limits its application range and service time. How to make ZrO2 fiber have the characteristics of high temperature and high strength is an urgent goal to be achieved.
[0003] In Chinese patent document CN103993387A, a method for preparing ultra-high temperature resistant kilometer-level continuous ZrO2 crystal fiber is disclosed. However, after high temperature treatment, the fiber has large grain size and low tensile strength. Moreover, after long-term high temperature treatment, the mechanical properties have been greatly reduced due to the growth of grains. Therefore, in order to obtain ZrO2 fibers with good mechanical properties, it is necessary to propose a scientific and effective method to inhibit the growth of grains.
[0004] CN106757525A discloses a method for producing crystal fibers, and the operating steps are as follows: (1) pulping: flexible silica fibers, magnesium aluminate fibers and zirconium oxide continuous fibers are mixed in proportion and slowly added to a slowly stirred slurry pool, and mixed with a binder solution in the slurry pool to form a zirconium oxide fiber slurry until the mixture is stirred evenly; (2) vacuum filtration molding: a mold is placed in a stirred slurry pool, a vacuum pump is turned on, and a fiberboard wet blank with a stable shape is obtained by vacuum filtration; (3) calcination: pretreatment is first performed at 2000°C for 5 hours, and then calcined at 2000°C for 15 hours to dry the fiberboard wet blank to a moisture content of less than 0.5%, and the shrinkage rates of the fiberboard wet blank in length, width and thickness directions are 1.10%, 1.02% and 1.80% respectively. CN107586143A discloses a high-performance zirconia fiberboard, characterized in that the components include the following components by weight: 100 parts of zirconia fiber, 3 to 6 parts of silica-alumina sol, 3 to 6 parts of tetraethyl orthosilicate, 8 to 10 parts of epoxy resin, and 1 to 2 parts of dispersant. The above-mentioned prior art only mixes components with different properties to obtain a fiberboard with improved performance, and cannot fundamentally solve the problem that zirconia continuous fiber inhibits grain growth and has poor mechanical properties at high temperatures.
[0005] In addition, CN111233445A discloses a high-temperature, high-strength, flexible zirconium oxide-silicon oxide fiber membrane and its preparation method and application. The method uses polyacetylacetonate zirconium as a zirconium source, a silane coupling agent as a silicon source, and polyethylene oxide as a spinning aid to prepare a zirconium-silicon polymer precursor spinning solution, obtain a precursor fiber membrane by electrostatic spinning, and obtain a high-temperature, high-strength, flexible zirconium oxide-silicon oxide fiber membrane by heat treatment. However, at a high temperature of more than 1300°C, silicon oxide is easily precipitated from the fiber membrane, resulting in a significant reduction in high-temperature mechanical properties. The mechanical strength of the fiber membrane at a high temperature of 1300°C is only 4.9MPa.
[0006] Therefore, how to ensure that the zirconia continuous fiber has excellent mechanical properties at high temperatures has become a technical problem that needs to be solved urgently. To this end, the present invention is proposed. Summary of the invention:
[0007] In view of the deficiencies of the existing technology and process, the present invention proposes a silicon-modified high-temperature high-strength zirconia continuous fiber and its preparation method and application, in particular, a high-temperature high-strength silicon-modified zirconia continuous fiber with a linear spinnable structure and a metal organic polymer as a precursor and its preparation method and application. The present invention introduces a silicon source into an organic zirconium source precursor and controls the ratio of the silicon source to the zirconium source within a reasonable range, so that the silicon-modified zirconia continuous fiber can inhibit the growth of zirconia grains under high temperature conditions of 1300°C to 1500°C, and prevent silicon precipitation, ultimately ensuring the good mechanical properties of the zirconia continuous fiber under high temperature conditions.
[0008] After high-temperature heat treatment, the precursor fiber prepared by the present invention forms a dual-phase structure of amorphous silicon oxide and tetragonal or cubic zirconium oxide. The amorphous silicon oxide is located between the zirconium oxide grains, which increases the diffusion energy barrier of atoms at the grain boundaries. The grain annealing and growth are delayed, and the grain size is reduced by 50%; at the same time, the filling of amorphous silicon oxide at the grain boundaries of the zirconium oxide grains reduces defects such as pores and reduces stress concentration under stress. The tensile strength of the fiber finally obtained can reach 2.0GPa to 3.0GPa, the radius of curvature is only 0.4mm to 1mm, and it can still maintain good mechanical properties after being treated at a high temperature of 1300℃ to 1500℃ for a long time.
[0009] The technical solution of the present invention is as follows:
[0010] Silicon modified high temperature high strength zirconia continuous fiber, the fiber is composed of zirconia grains and silicon oxide, the silicon oxide exists at the grain boundary of the zirconia grains, and the silicon oxide content accounts for 2%-10% of the total molar amount of zirconia and silicon oxide, and more preferably 4%-8%.
[0011] According to the present invention, preferably, in the silicon-modified high-temperature and high-strength zirconia continuous fibers, silicon oxide exists in the form of amorphous silicon oxide.
[0012] According to the present invention, preferably, in the silicon-modified high-temperature high-strength zirconia continuous fibers, the average size of the zirconia grains is 10 nm to 45 nm.
[0013] According to the present invention, preferably, after the silicon-modified high-temperature high-strength zirconia continuous fiber is subjected to a high-temperature treatment at 1300°C to 1500°C, the tensile strength of the fiber single fiber is 2.0GPa to 3.0GPa, and the radius of curvature is 0.4 to 1mm.
[0014] According to the present invention, preferably, the diameter of the silicon-modified high-temperature high-strength zirconia continuous fiber is 5 μm to 25 μm, and the continuous length of the single fiber can reach more than a kilometer.
[0015] According to the present invention, the method for preparing the above-mentioned silicon-modified high-temperature high-strength zirconia continuous fiber comprises the following steps:
[0016] (1) dissolving a zirconium source in a solvent, adding a silicon source, adding or not adding a stabilizer, stirring and dissolving to obtain a precursor solution; concentrating and aging the precursor solution to obtain a precursor spinning sol;
[0017] (2) dry spinning the precursor spinning sol to obtain a precursor continuous fiber;
[0018] (3) The precursor continuous fiber is subjected to pressure analysis, low-temperature steam treatment and high-temperature heat treatment sintering to obtain high-temperature and high-strength silicon-modified zirconia continuous fiber.
[0019] According to the present invention, preferably, the zirconium source in step (1) is poly(acetylacetonate) zirconium (PAZ);
[0020] The stabilizer is yttrium nitrate or yttrium polyacetylacetonate;
[0021] The silicon source is methyl orthosilicate or silane, and more preferably, the silane is methyltrimethoxysilane, dimethyldiethoxysilane, methyltriethoxysilane or γ-chloropropyltriethoxysilane;
[0022] Preferably, the solvent is one or a mixture of two or more of anhydrous methanol, anhydrous ethanol, acetone, and N,N-dimethylformamide.
[0023] According to the present invention, preferably, the molar ratio of the silicon source to the zirconium source in step (1) is 1:49 to 1:9, and more preferably 1:24 to 1:11.5.
[0024] According to the present invention, preferably, the aging temperature in step (1) is 40-60° C., the aging time is 1-6 days, and the viscosity of the sol after aging is 450-600 Pa·s.
[0025] According to the present invention, preferably, the dry spinning in step (2) is: the spinning solution is pressurized to 2-3 MPa by means of a steel bottle nitrogen or a metering pump, and the spinneret hole diameter is 0.04-0.1 mm.
[0026] According to the present invention, preferably, the air temperature of the dry spinning in step (2) is 15-35° C., and the air humidity is 30%-60%.
[0027] According to the present invention, preferably, in step (3), after the atmosphere is introduced, the pressure is controlled at 15 atmospheres, and the temperature is raised to 200° C. for analysis.
[0028] According to the present invention, preferably, in step (3), the temperature is raised to 1300-1500° C. at a heating rate of 10-100° C. / min for sintering.
[0029] According to the preparation method of the present invention, a preferred embodiment comprises the following steps:
[0030] (1) Preparing a precursor sol: dissolving a zirconium source in a solvent, adding a silicon source, adding or not adding a stabilizer, stirring and dissolving to obtain a precursor solution; the zirconium source is polyacetylacetonate zirconium PAZ, and the stabilizer is yttrium nitrate; the solvent is one or a mixture of two or more of anhydrous methanol, anhydrous ethanol, acetone, and N,N-dimethylformamide; the silicon source is methyl orthosilicate or silane; in the spinning solution, the molar content of the silicon source is 2-10%, the molar content of the zirconium source is 98%-90%, the molar ratio of the stabilizer to the zirconium source is 1:10-1:49, the volume ratio of the organic solvent to the zirconium source is 1:1.5-1:2.5, and the mass ratio of the zirconium source to the solvent is 1:3-1:5;
[0031] The precursor solution prepared above is concentrated under reduced pressure to form a transparent, spinnable sol with a suitable viscosity; the spinnable sol with a suitable viscosity is poured into a spinning barrel, and then the spinning barrel is placed in an oven at 40 to 60° C. for aging to make the sol uniform and stable;
[0032] (2) Dry spinning to prepare precursor continuous gel fibers: The precursor sol obtained in step (1) is used to obtain precursor continuous fibers using dry spinning technology, wherein the spinning bundle is 40 to 1000 fibers and the spinneret hole diameter is 0.04 to 0.1 mm;
[0033] (3) Heat treatment and sintering to prepare silicon-modified zirconia continuous fibers: The precursor continuous fibers are placed in a pressure vessel preheated to 90-130°C, the pressure is controlled at 15 atmospheres after the atmosphere is introduced, and the temperature is raised to 200°C for decomposition treatment for 20 minutes to 1 hour, so that most of the organic matter in the precursor fibers is decomposed; the fibers after pressure decomposition treatment are placed in a sintering furnace for heat treatment in the presence of steam, wherein the steam is water vapor, and the temperature is raised to 500-800°C at a heating rate of 0.1-5°C / min, so that the organic matter in the precursor fibers is decomposed and the inorganic matter is crystallized and converted into continuous silicon-modified zirconia fibers; the temperature is raised to 1300-1500°C at a heating rate of 10-100°C / min, and sintered to obtain continuous zirconia crystal fibers with a diameter of 5-25 μm and a single fiber continuous length of more than one kilometer.
[0034] According to the present invention, the poly acetylacetonate zirconium (PAZ) can be prepared by referring to the prior art, which can be found in Chinese patent document CN 1459418A.
[0035] According to the present invention, silicon-modified high-temperature high-strength zirconia continuous fiber can be used for structural reinforcement materials, high-temperature flexible refractory materials, fire-fighting insulation materials and chemical corrosion-resistant materials because of its excellent properties such as high melting point, high hardness, good chemical stability and good mechanical properties at high temperatures above 1300°C.
[0036] According to the present invention, the application of silicon-modified high-temperature high-strength zirconia continuous fiber is used as a structural reinforcement material, a high-temperature flexible refractory material, a fire-fighting heat-insulating material and a chemical corrosion-resistant material. It is used in the fields of aerospace, automobiles, high-speed rail, etc.
[0037] The advantages of the present invention compared with the prior art are as follows:
[0038] 1. The present invention introduces a silicon source into an organic zirconium source precursor and controls the ratio of the silicon source to the zirconium source within a reasonable range, so that the silicon-modified zirconia continuous fiber can inhibit the growth of zirconia grains under high temperature conditions of 1300°C to 1500°C and prevent silicon precipitation, ultimately ensuring the good mechanical properties of the zirconia continuous fiber under high temperature conditions of 1300°C to 1500°C.
[0039] The high-temperature and high-strength silicon-modified zirconia continuous fiber of the present invention has uniform diameter, compact structure, small grain size, tensile strength as high as 2.0-3.0 GPa, and a curvature radius of only 0.4-1 mm.
[0040] 2. The precursor sol prepared by the present invention has linear spinnability and can realize controllable viscosity. The continuous length of the spun precursor fiber monofilament can reach several thousand meters.
[0041] 3. The present invention can achieve controllable decomposition of organic matter through pressure analysis and low-temperature steam treatment, effectively improve the mechanical properties of the fiber, and achieve fiber densification at high temperature through a controllable heating rate, with the final grain size being only about 40nm.
[0042] 4. The silicon-modified zirconia continuous fiber prepared by the present invention can be used as refractory materials, heat insulation materials, fiber reinforcement materials, and applied in the fields of aerospace, automobiles, high-speed rail, etc. The present invention has the characteristics of simple method, low cost, no pollution, stable fiber quality, etc. Description of the drawings:
[0043] Figure 1 is the XED spectrum of the silicon-modified zirconia continuous fiber obtained in Example 1 sintered at 1500°C;
[0044] Figure 2 is a SEM image of the silicon-modified zirconia continuous fiber obtained in Example 1 sintered at 1500° C.;
[0045] Figure 3 is a STEM image of the silicon-modified zirconia continuous fiber obtained in Example 1 sintered at 1500° C.;
[0046] Figure 4 is a STEM-EDS image of the silicon-modified zirconia continuous fiber obtained in Example 1 sintered at 1500° C.;
[0047] Figure 5 is a particle size distribution diagram of the silicon-modified zirconia continuous fiber obtained in Example 1 after sintering at 1500° C.;
[0048] Figure 6 This is the stress-strain diagram of the silicon-modified zirconia continuous fiber obtained in Example 1 after sintering at 1500°C. Specific embodiment:
[0049] The present invention will be further described below through specific embodiments in conjunction with the accompanying drawings, but is not limited thereto.
[0050] Embodiment 1:
[0051] A method for preparing high-temperature and high-strength silicon-modified zirconia continuous fibers comprises the following steps:
[0052] (1) Preparation of precursor sol: Dissolve 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) in 200 g of anhydrous ethanol, then add 5.3 g of dimethyldiethoxysilane to the above solution, wherein the Si:Zr molar ratio is 8:92, and continue stirring for 1 hour. The above solution is concentrated under reduced pressure at 40°C to form a transparent, spinnable sol with a suitable viscosity. The precursor solution prepared above is concentrated under reduced pressure to form a transparent, spinnable sol with a suitable viscosity. Pour the spinnable sol with a suitable viscosity into a spinning barrel, and then place the spinning barrel in a 60°C oven for aging to make the sol uniform and stable.
[0053] (2) Dry spinning to prepare continuous precursor fibers: The precursor sol obtained in step 1 is used to obtain continuous precursor fibers by dry spinning technology. The liquid material tank containing the spinning sol is vacuum degassed for 10 minutes. Under the conditions of temperature of 20°C and relative humidity of 80%, a pressure of 3.5MPa is applied to the spinning solution by means of a cylinder nitrogen or a metering pump to make it spray out from a 50-hole niobium-tantalum alloy spinning plate with a pore size of 0.05mm. After drawing and collecting, a transparent, orderly arranged, continuous precursor fiber with a diameter of 30μm is obtained.
[0054] (3) Heat treatment and sintering to prepare silicon-modified zirconia continuous fibers: The precursor continuous fibers are placed in a pressure vessel preheated to 110°C, and the pressure is controlled at 15 atmospheres after the atmosphere is introduced. The temperature is raised to 200°C and the treatment time is 1 hour, so that the organic matter in the precursor fibers is decomposed. The fibers after pressure decomposition treatment are placed in a sintering furnace for heat treatment, and the temperature is raised to 700°C at a heating rate of 5°C / min, so that the organic matter in the precursor fibers is decomposed and the inorganic matter is crystallized and converted into continuous silicon-modified zirconia fibers. The temperature is raised to 1500°C at a heating rate of 10°C / min and sintered to obtain continuous zirconia crystal fibers with a diameter of 22 μm and a single fiber continuous length of more than one kilometer.
[0055] The XRD spectrum of the silicon-modified zirconia continuous fiber obtained in this example after sintering at 1500°C is as follows: Figure 1 It can be seen that the fiber phase is tetragonal zirconia, and no diffraction peak of silicon dioxide is found, indicating that silicon oxide is amorphous in the fiber.
[0056] The SEM image of the silicon-modified zirconia continuous fiber obtained in this example after sintering at 1500°C is shown in FIG. Figure 2 , it can be seen that the fiber diameter is uniform and complete, and there are no obvious cracks on the surface.
[0057] The STEM image of the silicon-modified zirconia continuous fiber obtained in this example after sintering at 1500°C ( Figure 3 )、STEM-EDS images( Figure 4 ), it can be seen that amorphous silicon oxide exists at the grain boundaries of zirconium oxide grains. This structure can inhibit the growth of grains at high temperatures and relieve stress concentration at grain boundaries.
[0058] The grain diameter statistics of the silicon-modified zirconia continuous fiber obtained in this example after sintering at 1500°C are shown in the figure below: Figure 5 , it can be seen that the grain size distribution is uniform and the average grain size is 38nm.
[0059] The stress-strain diagram of the silicon-modified zirconia continuous fiber obtained in this example after sintering at 1500°C is shown in Figure 6 It can be seen that the fiber is linearly broken and the average tensile strength can reach 2.8GPa.
[0060] Embodiment 2:
[0061] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) were dissolved in 200 g of anhydrous ethanol according to a molar ratio of Si:Zr=2:98, and 0.5 g of methyl orthosilicate was added to the above solution, and stirring was continued for 1 hour.
[0062] The silicon-modified zirconia continuous fibers obtained in this example have uniform diameters, smooth and complete surfaces, and an average tensile strength of 2.2 GPa.
[0063] Embodiment 3:
[0064] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) were dissolved in 200 g of anhydrous ethanol according to a molar ratio of Si:Zr=4:96, and 2.3 g of methyltrimethoxysilane was added to the above solution, and stirring was continued for 1 hour.
[0065] The silicon-modified zirconia continuous fibers obtained in this example have uniform diameters, smooth and complete surfaces, and an average tensile strength of 2.6 GPa.
[0066] Embodiment 4:
[0067] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) was dissolved in 200 g of anhydrous ethanol at a molar ratio of Si:Zr=6:94, and 6.3 g of γ-chloropropyltriethoxysilane was added to the above solution, and stirring was continued for 1 hour.
[0068] The silicon-modified zirconia continuous fibers obtained in this example have uniform diameters, smooth and complete surfaces, and an average tensile strength of 2.7 GPa.
[0069] Embodiment 5:
[0070] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) were dissolved in 200 g of anhydrous ethanol according to a molar ratio of Si:Zr=8:92, and 6.4 g of methyltriethoxysilane was added to the above solution, and stirring was continued for 1 hour.
[0071] The silicon-modified zirconia continuous fibers obtained in this example have uniform diameters, smooth and complete surfaces, and a tensile strength of 3.0 GPa.
[0072] Embodiment 6:
[0073] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) were dissolved in 200 g of anhydrous ethanol according to a molar ratio of Si:Zr=10:90, and 6.2 g of methyltrimethoxysilane was added to the above solution, and stirring was continued for 1 hour.
[0074] The silicon-modified zirconia continuous fibers obtained in this example have uniform diameters, smooth and complete surfaces, and a tensile strength of 2.5 GPa.
[0075] Embodiment 7:
[0076] As described in Example 1, the difference is that in step (2), the diameter of the spinneret hole is 0.04 mm, the number of spinneret holes is 500, the pressure is 3.0 MPa, the spinning temperature is 30°C, and the precursor fiber is stretched in multiple stages to obtain a smoother, wrinkle-free continuous fiber.
[0077] Embodiment 8:
[0078] As described in Example 1, the difference is that the fiber after the pressure analysis treatment in step (3) is placed in a sintering furnace for heat treatment, and the temperature is increased to 600° C. at a heating rate of 1° C. / min.
[0079] Embodiment 9:
[0080] The difference is that the fiber after the pressure analysis treatment in step (3) is placed in a sintering furnace for heat treatment, heated to 800°C at a heating rate of 5°C / min, kept at a constant temperature for 2 hours, the steam is turned off, and the temperature is naturally cooled to room temperature.
[0081] Embodiment 10:
[0082] As described in Example 1, the difference is that during the high temperature heat treatment in step (3), the temperature is raised to 1300° C. at a heating rate of 10° C. / min, and the fiber grain size finally obtained is smaller.
[0083] Embodiment 11:
[0084] As described in Example 1, the difference is that during the high-temperature heat treatment in step (3), the temperature is raised to 1500°C at a heating rate of 100°C / min, and the grain size of the fiber finally obtained is reduced and the fiber strength is improved.
[0085] Comparative Example 1:
[0086] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) were dissolved in 200 g of anhydrous ethanol at a molar ratio of Si:Zr=1:1, and 60.9 g of dimethyldiethoxysilane was added to the above solution, and stirring was continued for 1 hour.
[0087] There are a large number of microcracks on the surface of the silicon-modified zirconia continuous fiber obtained in this comparative example, and the fiber strength is greatly reduced. This is mainly because the decomposition intensity of dimethyldiethoxysilane is increased, and the oxidation and combustion of carbon produces gases that form a large number of pores and cracks inside the fiber, which has a negative impact on the mechanical properties of the fiber and is not conducive to the high strength and uniformity of the fiber.
[0088] After high-temperature treatment at 1500°C, the tensile strength of the fiber monofilament in this comparative example is 0.8 GPa.
[0089] Comparative Example 2:
[0090] As described in Example 1, except that in step (1), 100 g of polyacetylacetonate zirconium (PAZ) and 10.06 g of yttrium nitrate hexahydrate (YCl3·6H2O) were dissolved in 200 g of anhydrous ethanol at a molar ratio of Si:Zr=15:85, and 16.07 g of tetraethyl orthosilicate was added to the above solution, and stirring was continued for 1 hour.
[0091] The silicon-modified zirconia continuous fibers obtained in this comparative example have uniform diameters, microcracks on the surface, and reduced strength.
[0092] After high-temperature treatment at 1500°C, the tensile strength of the fiber monofilament in this comparative example is 1.2 GPa.
[0093] Comparative Example 3:
[0094] As described in Example 1, except that in step (1), the molar ratio of Si:Zr=1:99 is followed.
[0095] The silicon-modified zirconia continuous fiber obtained in this comparative example has a uniform diameter, an average grain size of 68nm, and a decreased strength. This is mainly because the amorphous silicon oxide content in the fiber is low, which reduces the inhibitory effect on the growth of zirconia grains. The grains grow and cannot achieve the requirements of high-temperature, high-strength and flexible performance.
[0096] After high-temperature treatment at 1500°C, the tensile strength of the fiber monofilament in this comparative example is 1.0 GPa.
[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Silicon-modified high-temperature high-strength zirconia continuous fiber, characterized in that: The fiber is composed of zirconium oxide grains and silicon oxide. The silicon oxide exists at the grain boundaries of the zirconium oxide grains. The silicon oxide content accounts for 2%-10% of the total molar amount of zirconium oxide and silicon oxide. The tensile strength of the fiber single wire is 2.0 GPa-3.0 GPa. Prepared as follows: (1) dissolving a zirconium source in a solvent, adding a silicon source, adding or not adding a stabilizer, stirring and dissolving to obtain a precursor solution; concentrating and aging the precursor solution to obtain a precursor spinning sol; the zirconium source is polyacetylacetonate zirconium, the silicon source is methyl orthosilicate or silane, and the solvent is one or a mixture of two or more of anhydrous methanol, anhydrous ethanol, acetone, and N,N-dimethylformamide; (2) dry spinning the precursor spinning sol to obtain precursor continuous fibers; (3) The precursor continuous fiber is subjected to pressure analysis, low-temperature steam treatment and high-temperature heat treatment sintering to obtain high-temperature and high-strength silicon-modified zirconia continuous fiber; the low-temperature steam treatment is to heat the pressure analysis to a temperature of 200°C for analysis; the high-temperature heat treatment sintering is to heat the temperature to 1300-1500°C at a heating rate of 10-100°C / min for sintering.
2. The silicon-modified high-temperature high-strength zirconia continuous fiber according to claim 1, characterized in that: In the silicon-modified high-temperature high-strength zirconia continuous fiber, the silicon oxide content accounts for 4%-8% of the total molar amount of zirconium oxide and silicon oxide.
3. The silicon-modified high-temperature high-strength zirconia continuous fiber according to claim 1, characterized in that: In the silicon-modified high-temperature and high-strength zirconia continuous fibers, silicon oxide exists in the form of amorphous silicon oxide.
4. The silicon-modified high-temperature high-strength zirconia continuous fiber according to claim 1, characterized in that: In the silicon-modified high-temperature and high-strength zirconia continuous fibers, the average size of the zirconia grains is 10 nm to 45 nm.
5. The silicon-modified high-temperature high-strength zirconia continuous fiber according to claim 1, characterized in that: Silicon modified high temperature and high strength zirconia continuous fiber, the radius of curvature is 0.4 to 1 mm.
6. The silicon-modified high-temperature high-strength zirconia continuous fiber according to claim 1, characterized in that: The diameter of the silicon-modified high-temperature high-strength zirconia continuous fiber is 5 μm to 25 μm, and the continuous length of the single fiber is 0 < ≤ 1000 meters or the continuous length of the single fiber is > 1000 meters.
7. The method for preparing the silicon-modified high-temperature high-strength zirconia continuous fiber according to any one of claims 1 to 6, comprising the following steps: (1) dissolving a zirconium source in a solvent, adding a silicon source, adding or not adding a stabilizer, stirring and dissolving to obtain a precursor solution; concentrating and aging the precursor solution to obtain a precursor spinning sol; the zirconium source is polyacetylacetonate zirconium, the silicon source is methyl orthosilicate or silane, and the solvent is one or a mixture of two or more of anhydrous methanol, anhydrous ethanol, acetone, and N,N-dimethylformamide; (2) dry spinning the precursor spinning sol to obtain precursor continuous fibers; (3) The precursor continuous fiber is subjected to pressure analysis, low-temperature steam treatment and high-temperature heat treatment sintering to obtain high-temperature and high-strength silicon-modified zirconia continuous fiber; the low-temperature steam treatment is to heat the pressure analysis to a temperature of 200°C for analysis; the high-temperature heat treatment sintering is to heat the temperature to 1300-1500°C at a heating rate of 10-100°C / min for sintering.
8. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: The stabilizer in step (1) is yttrium nitrate or yttrium polyacetylacetonate.
9. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: The silane described in step (1) is methyltrimethoxysilane, dimethyldiethoxysilane, methyltriethoxysilane or γ-chloropropyltriethoxysilane.
10. The method for preparing silicon-modified high-temperature and high-strength zirconia continuous fibers according to claim 7, characterized in that: The molar ratio of the silicon source to the zirconium source in step (1) is 1:49 to 1:
9.
11. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: In step (1), the molar ratio of the silicon source to the zirconium source is 1:24 to 1:11.
5.
12. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: The aging temperature in step (1) is 40-60° C., the aging time is 1-6 days, and the viscosity of the sol after aging is 450-600 Pa·s.
13. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: In step (2), the dry spinning method is as follows: the spinning solution is pressurized to 2-3 MPa by means of a steel bottle nitrogen or a metering pump, and the spinneret hole diameter is 0.04-0.1 mm.
14. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: In step (2), the air temperature of dry spinning is 15-35° C., and the air humidity is 30%-60%.
15. The method for preparing silicon-modified high-temperature high-strength zirconia continuous fibers according to claim 7, characterized in that: After the atmosphere is introduced in step (3), the pressure is controlled at 15 atmospheres.
16. The application of the silicon-modified high-temperature high-strength zirconia continuous fiber according to any one of claims 1 to 6 is used as a structural reinforcement material, a high-temperature flexible refractory material, a fire-fighting heat-insulating material and a chemical corrosion-resistant material, and is applied to the fields of aerospace, automobiles and high-speed rail.
Citation Information
Patent Citations
Method for preparing ultrahigh-temperature-resistant kilometric continuous zirconia crystal fiber
CN103993387A
Production method of crystal fibers
CN106757525A
Zirconia fiber insulation board and preparation method thereof
CN107586143A
High-temperature high-strength flexible zirconium oxide-silicon oxide fiber membrane as well as preparation method and application thereof
CN111233445A
Method and equipment of preparing high performance zirconium oxide continuous fiber
CN1459418A