A high-strength dense silicon nitride ceramic material and preparation method thereof
By adding carbon sources to silicon nitride ceramic materials and using ultrasonic treatment and ball milling technology, combined with specific sintering conditions, the problem of poor density of silicon nitride ceramic materials is solved, significantly improving its mechanical strength and mechanical properties, and expanding its Scope of application.
Patent Information
- Application Number
- CN202310900940.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-07-21
AI Technical Summary
The poor density of silicon nitride ceramic materials leads to the inability to meet the application requirements in high-demand fields.
By sonicating the silicon nitride powder, carbon source and sintering aid in anhydrous ethanol, a dispersion material is obtained, which is then ball-milled in a ball mill and dried in a vacuum drying box, followed by sintering in a graphite mold, using a specific The temperature increase and cooling rate are sintered to form a high-strength dense silicon nitride ceramic material.
It significantly improves the mechanical properties and denseness of silicon nitride ceramic materials, and improves its application range in high-demand fields, including thermal shock resistance, wear resistance and acid and alkali corrosion resistance.
Smart Images

Figure CN116947504B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of silicon nitride ceramic materials, and in particular to a high-strength and dense silicon nitride ceramic material and a preparation method thereof. Background Art
[0002] Silicon nitride ceramic materials have excellent high temperature resistance, corrosion resistance and mechanical properties, so they have broad application prospects in aerospace, energy, electronics and other fields. However, silicon nitride is a covalent bond compound with a low atomic self-diffusion coefficient, low volume diffusion and grain boundary diffusion rates, which makes it difficult to densify silicon nitride ceramics during sintering, so silicon nitride materials have poor sinterability. Therefore, traditional silicon nitride ceramic materials have problems such as low strength and poor density, which limits their application in some high-demand fields.
[0003] How to improve the poor density of existing silicon nitride ceramic materials, which results in their mechanical strength failing to meet the application requirements in high-demand fields, is the key to the present invention. Therefore, a high-strength and dense silicon nitride ceramic material and its preparation method are urgently needed to solve the above problems. Summary of the invention
[0004] In order to overcome the above technical problems, the purpose of the present invention is to provide a high-strength and dense silicon nitride ceramic material and a preparation method thereof: silicon nitride powder, a carbon source, and a sintering aid are added to anhydrous ethanol for ultrasonic treatment to obtain a dispersed material, the dispersed material is added to a ball mill for ball milling to obtain a ball-milled material, the ball-milled material is placed in a vacuum drying oven for drying, then crushed and sieved to obtain a dry material, the dry material is added to a graphite mold for sintering, and then cold-cut with the furnace to obtain a high-strength and dense silicon nitride ceramic material, which solves the problem that the existing silicon nitride ceramic material has poor density, resulting in its mechanical strength not being able to meet the application requirements of high-demand fields.
[0005] The purpose of the present invention can be achieved by the following technical solutions:
[0006] A method for preparing a high-strength and dense silicon nitride ceramic material comprises the following steps:
[0007] Step 1: Weigh 60-80 parts of silicon nitride powder, 5-25 parts of carbon source, 10-15 parts of sintering aid and 220-250 parts of anhydrous ethanol according to weight parts and set aside;
[0008] Step 2: Add silicon nitride powder, carbon source and sintering aid into anhydrous ethanol, and then perform ultrasonic treatment for 10-15min at an ultrasonic power of 300-320W to obtain a dispersed material;
[0009] Step 3: Add the dispersed material into a ball mill, add zirconium dioxide ball milling medium at a ball-to-material mass ratio of 3-4:1, and then ball mill for 20-30 hours at a rotation speed of 300-400 r / min to obtain a ball mill;
[0010] Step 4: Place the ball mill in a vacuum drying oven and dry at 100-110°C for 10-15 hours, then cool to room temperature, and crush through a 100-125 mesh sieve to obtain a dry material;
[0011] Step 5: Add the dried material into the graphite mold, introduce argon protection, and then heat it to a sintering temperature of 1500-1550℃ at a heating rate of 8-10℃ / min under a sintering pressure of 10-15MPa, and sinter for 1-1.5h. Then heat it to 1750-1800℃ and sinter for 3-4h. Then cool it to 1150-1200℃ at a cooling rate of 10-12℃ / min and keep it for 1-2h. Then cool it with the furnace to obtain a high-strength and dense silicon nitride ceramic material.
[0012] As a further solution of the present invention: the sintering aid is one of lanthanum oxide, yttrium oxide, magnesium oxide, and aluminum oxide, or a mixture of two or more of them in any proportion.
[0013] As a further solution of the present invention: the sintering aid is a mixture of lanthanum oxide and yttrium oxide in a molar ratio of 1:1.
[0014] As a further solution of the present invention: the sintering aid is a mixture of yttrium oxide and aluminum oxide in a molar ratio of 1:1.
[0015] As a further solution of the present invention: the sintering aid is a mixture of yttrium oxide, aluminum oxide and magnesium oxide in a mass ratio of 4:3:3.
[0016] As a further solution of the present invention: the silicon nitride powder is prepared by the following steps:
[0017] Add silicon dioxide powder and carbon powder to a planetary ball mill, ball mill for 20-30 hours at a rotation speed of 300-400r / min, then add to a tubular furnace, introduce nitrogen and maintain the nitrogen flow rate at 1-1.5L / min, heat to 1600-1620°C at a heating rate of 5-8°C / min, calcine for 2-2.5 hours, then cool to 600-620°C at a cooling rate of 3-5°C / min, keep warm for 4-5 hours, and then cool with the furnace to obtain silicon nitride powder.
[0018] As a further solution of the present invention: the usage ratio of the silicon dioxide powder and the carbon powder is 0.1 mol:0.35 mol.
[0019] As a further solution of the present invention: the carbon source is prepared by the following steps:
[0020] Step s1: D-glucosamine, sodium nitrite, potassium carbonate and deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and acryloyl chloride is added dropwise while stirring at a temperature of -5-0°C and a stirring rate of 300-400 r / min, and the dropping rate is controlled to be 1-2 drops / s. After the dropwise addition is completed, stirring and reacting for 2-3 hours, and then heating to 25-30°C and stirring and reacting for 20-30 hours. After the reaction is completed, the reaction product is poured into anhydrous ethanol, and then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain intermediate 1;
[0021] The reaction principle is as follows:
[0022]
[0023] Step s2: Sodium hydrosulfide and deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction at a temperature of 25-30°C and a stirring rate of 300-400 r / min for 20-30 min, and then a pH adjuster, a catalyst and a hydrolysis inhibitor are added and the stirring reaction is continued for 10-15 min, and then the temperature is raised to 60-65°C and γ-chloropropyltriethoxysilane is added dropwise while stirring, and the dropping rate is controlled to 1-2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 8-10 h. After the reaction is completed, the reaction product is cooled to room temperature, and then allowed to stand for stratification, and the organic phase is distilled under reduced pressure, and the fraction with a vacuum degree of 0.099 MPa and a temperature of 78-80°C is collected to obtain intermediate 2;
[0024] The reaction principle is as follows:
[0025]
[0026] Step s3: Add intermediate 1, intermediate 2, azobisisobutyronitrile and N,N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 15-20 minutes at a temperature of 5-10°C and a stirring rate of 300-400r / min, then raise the temperature to reflux and continue stirring the reaction for 6-8 hours. After the reaction is completed, the reaction product is cooled to room temperature, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a carbon source.
[0027] The reaction principle is as follows:
[0028]
[0029] As a further solution of the present invention: the dosage ratio of the D-glucosamine, sodium nitrite, potassium carbonate, deionized water and acryloyl chloride in step s1 is 4-4.5 g: 0.08-0.1 g: 2.8-3.0 g: 15-20 mL: 1.8-2.0 mL.
[0030] As a further scheme of the present invention: the usage ratio of the sodium hydrosulfide, deionized water, pH regulator, catalyst, hydrolysis inhibitor and γ-chloropropyltriethoxysilane in step s2 is 8.5g:100-120mL:2-3g:5-6g:1-1.5g:8-12g, the pH regulator is sodium dihydrogen phosphate, the catalyst is dodecyldimethylbenzylammonium chloride, and the hydrolysis inhibitor is pentaerythritol.
[0031] As a further solution of the present invention: the usage ratio of the intermediate 1, intermediate 2, azobisisobutyronitrile and N,N-dimethylformamide in step s3 is 0.1 mol: 0.1 mol: 0.15-0.35 g: 120-150 mL.
[0032] As a further solution of the present invention: a high-strength dense silicon nitride ceramic material comprises the following components in parts by weight:
[0033] 60-80 parts of silicon nitride powder, 5-25 parts of carbon source, 10-15 parts of sintering aid and 220-250 parts of anhydrous ethanol.
[0034] Beneficial effects of the present invention:
[0035] The invention discloses a high-strength and dense silicon nitride ceramic material and a preparation method thereof. The method comprises the following steps: adding silicon nitride powder, a carbon source and a sintering aid to anhydrous ethanol for ultrasonic treatment to obtain a dispersed material, adding the dispersed material to a ball mill to obtain a ball milled material, placing the ball milled material in a vacuum drying oven for drying, then crushing and sieving to obtain a dried material, adding the dried material to a graphite mold for sintering, and then cold cutting with a furnace to obtain a high-strength and dense silicon nitride ceramic material. The preparation method firstly uses silicon dioxide powder and carbon powder to pass nitrogen at high temperature for calcination, so that the following reaction occurs: SiO 2 +C+N 2 →Si 3 N 4 +CO, to produce silicon nitride, Si 3 N 4 The central Si atom is covalently bonded to the four surrounding N atoms, with strong bonding ability, and a three-dimensional spatial network structure is formed between the crystal phases. 3 N 4The material has many excellent properties such as excellent mechanical properties, thermal shock resistance, high wear resistance, acid and alkali corrosion resistance, etc. 3 N 4 During the sintering process, carbon source is added to the sintered silicon nitride ceramic material, and silicon carbide can be introduced into the sintered silicon nitride ceramic material. The extremely strong covalent bond of SiC determines its excellent properties, such as hardness second only to diamond, high compressive strength, low expansion coefficient, wear resistance, high temperature resistance and chemical corrosion resistance. Since the density of silicon nitride is almost the same as that of silicon carbide ceramics, silicon nitride and silicon carbide ceramics can be sintered into a composite ceramic of dispersed phase and continuous phase in different proportions. The structure of this composite ceramic material is interwoven with each other and has high density. SiC particles or whiskers have a strong bond with Si 3 N 4 The matrix material has various strengthening and toughening effects, and the prepared composite material has better 3 N 4 Or the performance of single-phase SiC is more prominent, therefore, the mechanical properties of the prepared silicon nitride ceramic material are greatly improved, expanding its scope of application;
[0036] In the process of preparing high-strength and dense silicon nitride ceramic materials, a carbon source is first prepared. First, the amino group on D-glucose is reacted with the chlorine atom on acryloyl chloride to introduce an alkenyl group to obtain intermediate 1. Then, sodium hydrosulfide reacts with γ-chloropropyltriethoxysilane to convert the chlorine atom on γ-chloropropyltriethoxysilane into a thiol group to obtain intermediate 2. Then, the alkenyl group on intermediate 1 and the thiol group on intermediate 2 undergo a click chemical reaction to obtain a carbon source. The molecular structure of the carbon source contains a large number of C atoms and siloxane groups. The siloxane groups are hydrolyzed to form silanols, which can be connected to the particle surfaces of silicon nitride powder and sintering aids during ball milling to improve their dispersibility and avoid their agglomeration, thereby making the ball milling effect better, making the particle size finer, and improving its density in the subsequent sintering process, thereby improving its strength. Moreover, the carbon source can provide carbon atoms, silicon atoms and oxygen atoms after calcination, so that the following reaction can occur: SiO 2 +C→SiC+CO,Si 3 N 4 +C→SiC+N 2 , thereby forming silicon carbide, so that the prepared silicon nitride ceramic material is a composite material of silicon nitride and silicon carbide, and ultimately the prepared silicon nitride ceramic material has excellent performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The present invention will be further described below in conjunction with the accompanying drawings.
[0038] Figure 1 The present invention is a process flow chart of a method for preparing a high-strength and dense silicon nitride ceramic material. DETAILED DESCRIPTION
[0039] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] Embodiment 1:
[0041] This embodiment is a method for preparing silicon nitride powder, comprising the following steps:
[0042] 0.1 mol of silicon dioxide powder and 0.35 mol of carbon powder were added to a planetary ball mill, ball-milled at a rotation speed of 300 r / min for 20 hours, then added to a tubular furnace, nitrogen was introduced and the nitrogen flow rate was maintained at 1 L / min, the temperature was increased to 1600°C at a heating rate of 5°C / min, and calcined for 2 hours, then cooled to 600°C at a cooling rate of 3°C / min and kept for 4 hours, and then cooled with the furnace to obtain silicon nitride powder.
[0043] Embodiment 2:
[0044] This embodiment is a method for preparing silicon nitride powder, comprising the following steps:
[0045] 0.1 mol silica powder and 0.35 mol carbon powder were added to a planetary ball mill, ball-milled at a rotation speed of 350 r / min for 25 h, then added to a tubular furnace, nitrogen was introduced and the nitrogen flow rate was maintained at 1.2 L / min, the temperature was increased to 1610°C at a heating rate of 6°C / min, and calcined for 2.2 h, then cooled to 610°C at a cooling rate of 4°C / min and kept for 4.5 h, and then cooled with the furnace to obtain silicon nitride powder.
[0046] Embodiment 3:
[0047] This embodiment is a method for preparing silicon nitride powder, comprising the following steps:
[0048] 0.1 mol silica powder and 0.35 mol carbon powder were added to a planetary ball mill, ball-milled at a rotation speed of 400 r / min for 30 hours, then added to a tubular furnace, nitrogen was introduced and the nitrogen flow rate was maintained at 1.5 L / min, the temperature was increased to 1620°C at a heating rate of 8°C / min, and calcined for 2.5 hours, then cooled to 620°C at a cooling rate of 5°C / min and kept for 5 hours, and then cooled with the furnace to obtain silicon nitride powder.
[0049] Embodiment 4:
[0050] This embodiment is a method for preparing a carbon source, comprising the following steps:
[0051] Step s1: 4 g of D-glucosamine, 0.08 g of sodium nitrite, 2.8 g of potassium carbonate and 15 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and 1.8 mL of acryloyl chloride was added dropwise while stirring at a temperature of -5°C and a stirring rate of 300 r / min, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the stirring reaction was continued for 2 h, and then the temperature was raised to 25°C and the stirring reaction was continued for 20 h. After the reaction was completed, the reaction product was poured into anhydrous ethanol, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0052] Step s2: 8.5 g of sodium hydrosulfide and 100 mL of deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction at a temperature of 25° C. and a stirring rate of 300 r / min for 20 min. Then, 2 g of a pH regulator, 5 g of a catalyst and 1 g of a hydrolysis inhibitor are added and the mixture is stirred for reaction for 10 min. Then, the mixture is heated to 60° C. and 8 g of γ-chloropropyltriethoxysilane is added dropwise while stirring. The dropping rate is controlled to be 1 drop / s. After the addition is completed, the mixture is stirred for reaction for 8 h. After the reaction is completed, the reaction product is cooled to room temperature, and then allowed to stand for stratification. The organic phase is distilled under reduced pressure, and a fraction with a vacuum degree of 0.099 MPa and a temperature of 78° C. is collected to obtain an intermediate 2; the pH regulator is sodium dihydrogen phosphate, the catalyst is dodecyldimethylbenzyl ammonium chloride, and the hydrolysis inhibitor is pentaerythritol;
[0053] Step s3: Add 0.1 mol intermediate 1, 0.1 mol intermediate 2, 0.15 g azobisisobutyronitrile and 120 mL N, N-dimethylformamide into a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, introduce nitrogen protection, stir the reaction at a temperature of 5°C and a stirring rate of 300 r / min for 15 min, then raise the temperature to reflux and continue stirring the reaction for 6 h. After the reaction is completed, the reaction product is cooled to room temperature, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a carbon source.
[0054] Embodiment 5:
[0055] This embodiment is a method for preparing a carbon source, comprising the following steps:
[0056] Step s1: 4.2 g of D-glucosamine, 0.09 g of sodium nitrite, 2.9 g of potassium carbonate and 18 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and 1.9 mL of acryloyl chloride was added dropwise while stirring at a temperature of -2°C and a stirring rate of 350 r / min, and the dropping rate was controlled to be 1 drop / s. After the addition was completed, the stirring reaction was continued for 2.5 h, and then the temperature was raised to 28°C and the stirring reaction was continued for 25 h. After the reaction was completed, the reaction product was poured into anhydrous ethanol, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0057] Step s2: 8.5 g of sodium hydrosulfide and 110 mL of deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for 25 min at a temperature of 28° C. and a stirring rate of 350 r / min. Then, 2.5 g of a pH regulator, 5.5 g of a catalyst and 1.2 g of a hydrolysis inhibitor are added, and the stirring reaction is continued for 12 min. Then, the temperature is raised to 62° C. and 10 g of γ-chloropropyltriethoxysilane is added dropwise while stirring. The dropping rate is controlled to be 1 drop / s. After the dropwise addition is completed, the stirring reaction is continued for 9 h. After the reaction is completed, the reaction product is cooled to room temperature, and then allowed to stand and stratify. The organic phase is distilled under reduced pressure, and a fraction with a vacuum degree of 0.099 MPa and a temperature of 79° C. is collected to obtain an intermediate 2; the pH regulator is sodium dihydrogen phosphate, the catalyst is dodecyldimethylbenzylammonium chloride, and the hydrolysis inhibitor is pentaerythritol;
[0058] Step s3: 0.1 mol intermediate 1, 0.1 mol intermediate 2, 0.25 g azobisisobutyronitrile and 135 mL N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 18 min at a temperature of 8°C and a stirring rate of 350 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 7 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a carbon source.
[0059] Embodiment 6:
[0060] This embodiment is a method for preparing a carbon source, comprising the following steps:
[0061] Step s1: 4.5 g of D-glucosamine, 0.1 g of sodium nitrite, 3.0 g of potassium carbonate and 20 mL of deionized water were added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and 2.0 mL of acryloyl chloride was added dropwise while stirring at a temperature of 0° C. and a stirring rate of 400 r / min. The dropping rate was controlled to be 2 drops / s. After the addition was completed, the stirring reaction was continued for 3 h, and then the temperature was raised to 30° C. and the stirring reaction was continued for 30 h. After the reaction was completed, the reaction product was poured into anhydrous ethanol, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain intermediate 1;
[0062] Step s2: 8.5 g of sodium hydrosulfide and 120 mL of deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction at a temperature of 30° C. and a stirring rate of 400 r / min for 30 min. Then, 3 g of a pH regulator, 6 g of a catalyst and 1.5 g of a hydrolysis inhibitor are added and the stirring reaction is continued for 15 min. Then, the temperature is raised to 65° C. and 12 g of γ-chloropropyltriethoxysilane is added dropwise while stirring. The dropping rate is controlled to be 2 drops / s. After the dropwise addition is completed, the stirring reaction is continued for 10 h. After the reaction is completed, the reaction product is cooled to room temperature, and then allowed to stand and stratify. The organic phase is distilled under reduced pressure, and a fraction with a vacuum degree of 0.099 MPa and a temperature of 80° C. is collected to obtain an intermediate 2; the pH regulator is sodium dihydrogen phosphate, the catalyst is dodecyldimethylbenzylammonium chloride, and the hydrolysis inhibitor is pentaerythritol;
[0063] Step s3: 0.1 mol intermediate 1, 0.1 mol intermediate 2, 0.35 g azobisisobutyronitrile and 150 mL N, N-dimethylformamide were added to a three-necked flask equipped with a stirrer, a thermometer, a gas duct and a reflux condenser, and nitrogen was introduced for protection. The reaction was stirred for 20 min at a temperature of 10°C and a stirring rate of 400 r / min, and then the temperature was raised to reflux and the stirring reaction was continued for 8 h. After the reaction was completed, the reaction product was cooled to room temperature, and then vacuum filtered, and the filtrate was rotary evaporated to remove the solvent to obtain a carbon source.
[0064] Embodiment 7:
[0065] See also Figure 1 As shown, this embodiment is a method for preparing a high-strength dense silicon nitride ceramic material, comprising the following steps:
[0066] Step 1: Weigh 60 parts of silicon nitride powder, 5 parts of carbon source, 10 parts of sintering aid and 220 parts of anhydrous ethanol according to weight parts for use; the silicon nitride powder is the silicon nitride powder in Example 1; the carbon source is the carbon source in Example 4; the sintering aid is a mixture of lanthanum oxide and yttrium oxide in a molar ratio of 1:1;
[0067] Step 2: adding silicon nitride powder, carbon source and sintering aid into anhydrous ethanol, and then ultrasonically treating for 10 min at an ultrasonic power of 300 W to obtain a dispersed material;
[0068] Step 3: Add the dispersed material into the ball mill, add zirconium dioxide ball milling medium at a ball-to-material mass ratio of 3:1, and then ball mill for 20 hours at a rotation speed of 300 r / min to obtain ball mill material;
[0069] Step 4: Place the ball mill in a vacuum drying oven and dry at 100°C for 10 hours, then cool to room temperature, and crush through a 100-mesh sieve to obtain a dry material;
[0070] Step 5: Add the dried material into the graphite mold, introduce argon protection, and then heat it to 1500℃ at a heating rate of 8℃ / min under a sintering pressure of 10MPa and sintering for 1h. Then heat it to 1750℃ and sinter it for 3h. Then cool it to 1150℃ at a cooling rate of 10℃ / min and keep it for 1h. Then cool it with the furnace to obtain a high-strength and dense silicon nitride ceramic material.
[0071] Embodiment 8:
[0072] See also Figure 1 As shown, this embodiment is a method for preparing a high-strength dense silicon nitride ceramic material, comprising the following steps:
[0073] Step 1: Weigh 70 parts of silicon nitride powder, 15 parts of carbon source, 12 parts of sintering aid and 235 parts of anhydrous ethanol according to weight parts for use; the silicon nitride powder is the silicon nitride powder in Example 2; the carbon source is the carbon source in Example 5; the sintering aid is a mixture of yttrium oxide and aluminum oxide in a molar ratio of 1:1;
[0074] Step 2: adding silicon nitride powder, carbon source and sintering aid into anhydrous ethanol, and then ultrasonically treating for 12 min at an ultrasonic power of 310 W to obtain a dispersed material;
[0075] Step 3: Add the dispersed material into the ball mill, add zirconium dioxide ball milling medium at a ball-to-material mass ratio of 3.5:1, and then ball mill for 25 hours at a rotation speed of 350 r / min to obtain ball mill material;
[0076] Step 4: Place the ball mill in a vacuum drying oven and dry at 105°C for 12 hours, then cool to room temperature, and crush through a 110-mesh sieve to obtain a dry material;
[0077] Step 5: Add the dried material into the graphite mold, introduce argon protection, and then heat it to 1525℃ at a heating rate of 9℃ / min under a sintering pressure of 12MPa, and sinter it for 1.2h. Then heat it to 1775℃ and sinter it for 3.5h. Then cool it to 1175℃ at a cooling rate of 11℃ / min and keep it for 1.5h. Then cool it with the furnace to obtain a high-strength and dense silicon nitride ceramic material.
[0078] Embodiment 9:
[0079] See also Figure 1 As shown, this embodiment is a method for preparing a high-strength dense silicon nitride ceramic material, comprising the following steps:
[0080] Step 1: Weigh 80 parts of silicon nitride powder, 25 parts of carbon source, 15 parts of sintering aid and 250 parts of anhydrous ethanol according to weight parts for use; the silicon nitride powder is the silicon nitride powder in Example 3; the carbon source is the carbon source in Example 6; the sintering aid is a mixture of yttrium oxide, aluminum oxide and magnesium oxide in a mass ratio of 4:3:3;
[0081] Step 2: adding silicon nitride powder, carbon source and sintering aid into anhydrous ethanol, and then ultrasonically treating for 15 min at an ultrasonic power of 320 W to obtain a dispersed material;
[0082] Step 3: Add the dispersed material into the ball mill, add zirconium dioxide ball milling medium at a ball-to-material mass ratio of 4:1, and then ball mill for 30 hours at a rotation speed of 400 r / min to obtain ball mill material;
[0083] Step 4: Place the ball mill in a vacuum drying oven and dry at 110°C for 15 hours, then cool to room temperature, and crush through a 125-mesh sieve to obtain a dry material;
[0084] Step 5: Add the dried material into the graphite mold, introduce argon protection, and then heat it to 1550℃ at a heating rate of 10℃ / min under a sintering pressure of 15MPa and keep it warm for 1.5h, then heat it to 1800℃ and keep it warm for 4h, then cool it to 1200℃ at a cooling rate of 12℃ / min and keep it warm for 2h, then cool it with the furnace to obtain high-strength and dense silicon nitride ceramic material.
[0085] Comparative Example 1:
[0086] The difference between Comparative Example 1 and Example 9 is that no carbon source is added.
[0087] Comparative Example 2:
[0088] The difference between Comparative Example 2 and Example 9 is that D-glucosamine is added instead of the carbon source.
[0089] The performance of the high-strength dense silicon nitride ceramic materials of Examples 7-9 and Comparative Examples 1-2 was tested, and the test results are as follows:
[0090]
[0091]
[0092] Referring to the data in the above table, it can be seen that adding D-glucosamine and carbon source can improve the bending strength of high-strength dense silicon nitride ceramic materials, and can also significantly improve their hardness and fracture toughness. Among them, the carbon source has the best improvement effect. Therefore, the addition of carbon source gives silicon nitride ceramic materials good mechanical properties and improves their mechanical strength.
[0093] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0094] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A method for preparing a high-strength and dense silicon nitride ceramic material, characterized in that: The following steps are involved: Step 1: Weigh 60-80 parts of silicon nitride powder, 5-25 parts of carbon source, 10-15 parts of sintering aid and 220-250 parts of anhydrous ethanol according to weight parts and set aside; Step 2: Add silicon nitride powder, carbon source and sintering aid into anhydrous ethanol, and then perform ultrasonic treatment for 10-15 minutes under the condition of ultrasonic power of 300-320W to obtain a dispersed material; Step 3: Add the dispersed material into a ball mill, add zirconium dioxide ball milling medium at a ball-to-material mass ratio of 3-4:1, and then ball mill for 20-30 hours at a rotation speed of 300-400 r / min to obtain a ball mill; Step 4: Place the ball mill in a vacuum drying oven and dry at 100-110°C for 10-15 hours, then cool to room temperature, and crush through a 100-125 mesh sieve to obtain a dry material; Step 5: Add the dried material into the graphite mold, introduce argon protection, then heat the sintering temperature to 1500-1550°C at a heating rate of 8-10°C / min under a sintering pressure of 10-15MPa, and sinter for 1-1.5h, then heat the temperature to 1750-1800°C and sinter for 3-4h, then cool the temperature to 1150-1200°C at a cooling rate of 10-12°C / min and keep it for 1-2h, then cool it with the furnace to obtain a high-strength and dense silicon nitride ceramic material; The carbon source is prepared by the following steps: Step s1: Add D-glucosamine, sodium nitrite, potassium carbonate and deionized water into a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, add acryloyl chloride dropwise while stirring at a temperature of -5-0°C and a stirring rate of 300-400r / min, and control the dropping rate to be 1-2 drops / s. After the dropwise addition is completed, continue to stir and react for 2-3 hours, then heat to 25-30°C and continue to stir and react for 20-30 hours. After the reaction is completed, pour the reaction product into anhydrous ethanol, then vacuum filter, and rotary evaporate the filtrate to remove the solvent to obtain intermediate 1; the dosage ratio of D-glucosamine, sodium nitrite, potassium carbonate, deionized water and acryloyl chloride is 4-4.5g:0.08-0.1g:2.8-3.0g:15-20mL:1.8-2.0mL; Step s2: Sodium hydrosulfide and deionized water are added to a three-necked flask equipped with a stirrer, a thermometer and a constant pressure dropping funnel, and the mixture is stirred for reaction for 20-30 minutes at a temperature of 25-30°C and a stirring rate of 300-400 r / min, and then a pH regulator, a catalyst and a hydrolysis inhibitor are added, and the stirring reaction is continued for 10-15 minutes, and then the temperature is raised to 60-65°C and γ-chloropropyltriethoxysilane is added dropwise while stirring, and the dropping rate is controlled to 1-2 drops / s. After the addition is completed, the stirring reaction is continued for 8-10 hours. After the reaction is completed, The reaction product is cooled to room temperature, and then allowed to stand for stratification, and the organic phase is distilled under reduced pressure, and a fraction with a vacuum degree of 0.099 MPa and a temperature of 78-80° C. is collected to obtain intermediate 2; the amount ratio of the sodium hydrosulfide, deionized water, pH regulator, catalyst, hydrolysis inhibitor and γ-chloropropyltriethoxysilane is 8.5 g: 100-120 mL: 2-3 g: 5-6 g: 1-1.5 g: 8-12 g, the pH regulator is sodium dihydrogen phosphate, the catalyst is dodecyl dimethyl benzyl ammonium chloride, and the hydrolysis inhibitor is pentaerythritol; Step s3: Add intermediate 1, intermediate 2, azobisisobutyronitrile and N,N-dimethylformamide to a three-necked flask equipped with a stirrer, a thermometer, an air duct and a reflux condenser, introduce nitrogen protection, stir the reaction for 15-20 minutes at a temperature of 5-10°C and a stirring rate of 300-400r / min, then raise the temperature to reflux and continue stirring the reaction for 6-8 hours. After the reaction is completed, the reaction product is cooled to room temperature, then vacuum filtered, and the filtrate is rotary evaporated to remove the solvent to obtain a carbon source; the amount ratio of the intermediate 1, intermediate 2, azobisisobutyronitrile and N,N-dimethylformamide is 0.1mol: 0.1mol: 0.15-0.35g: 120-150mL.
2. The method for preparing a high-strength dense silicon nitride ceramic material according to claim 1, characterized in that: The sintering aid is one of lanthanum oxide, yttrium oxide, magnesium oxide and aluminum oxide, or a mixture of two or more of them in any proportion.
3. The method for preparing a high-strength dense silicon nitride ceramic material according to claim 2, characterized in that: The sintering aid is a mixture of lanthanum oxide and yttrium oxide in a molar ratio of 1:
1.
4. The method for preparing a high-strength dense silicon nitride ceramic material according to claim 2, characterized in that: The sintering aid is a mixture of yttrium oxide and aluminum oxide in a molar ratio of 1:
1.
5. The method for preparing a high-strength dense silicon nitride ceramic material according to claim 2, characterized in that: The sintering aid is a mixture of yttrium oxide, aluminum oxide and magnesium oxide in a mass ratio of 4:3:
3.
6. The method for preparing a high-strength dense silicon nitride ceramic material according to claim 1, characterized in that: The silicon nitride powder is prepared by the following steps: Add silicon dioxide powder and carbon powder to a planetary ball mill, ball mill for 20-30 hours at a rotation speed of 300-400r / min, then add to a tubular furnace, introduce nitrogen and maintain the nitrogen flow rate at 1-1.5L / min, heat to 1600-1620℃ at a heating rate of 5-8℃ / min, calcine for 2-2.5h, then cool to 600-620℃ at a cooling rate of 3-5℃ / min, keep warm for 4-5h, and then cool with the furnace to obtain silicon nitride powder.
7. The method for preparing a high-strength dense silicon nitride ceramic material according to claim 6, characterized in that: The usage ratio of the silicon dioxide powder and the carbon powder is 0.1 mol:0.35 mol.
8. A high-strength dense silicon nitride ceramic material prepared by the method for preparing a high-strength dense silicon nitride ceramic material according to any one of claims 1 to 7, characterized in that: It includes the following components by weight: 60-80 parts of silicon nitride powder, 5-25 parts of carbon source, 10-15 parts of sintering aid and 220-250 parts of anhydrous ethanol.