A kind of aerogel ceramic coating and its preparation process

By combining modified polyimide aerogel and fluoro-containing silicone, a stable nano-scale pore structure is formed, which solves the structural instability of aerogel ceramic coatings, and improves its hardness, impact resistance and Thermal insulation performance achieves more efficient thermal insulation and fire protection.

CN117304800BActive Publication Date: 2024-11-05JIAXING FREBANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311270931.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-28
Publication Date
2024-11-05
Estimated Expiration
2043-09-28

AI Technical Summary

Technical Problem

The structural instability of aerogel ceramic coatings leads to poor thermal insulation and fire resistance and insufficient mechanical properties, which are difficult to improve in practical applications.

Method used

Using modified polyimide aerogel as the main component, through specific molar ratios and structural design, combining fluorosiloxane and polyphenylmethane polyamines to form a stable nano-scale pore structure, enhancing the coating. Hardness and impact resistance while reducing thermal conductivity.

Benefits of technology

It significantly improves the hardness, scrub resistance, acid and alkali resistance of ceramic coatings, and effectively reduces thermal conductivity, forming a more stable coating, suitable for high-performance thermal insulation and fire-resistant materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The invention provides a ceramic coating containing modified polyimide aerogel and a preparation process thereof. The modified polyimide aerogel is prepared by using a diamine compound with a special side chain as one of the diamine monomers and adding fluorinated siloxane, thereby improving the porous structure stability of the polyimide aerogel and achieving the effects of improving the hydrophobicity of the polyimide aerogel and reducing the shrinkage rate. The modified polyimide aerogel is added into the ceramic coating, so that the coating base paint has a low shrinkage rate during curing and is not easy to form shrinkage holes. The formed coating has excellent acid and alkali resistance and still has good adhesion after multiple washing and rubbing. At the same time, its thermal conductivity is low, and it has good heat insulation while being fireproof and non-combustible. It can be used in many high-temperature working environments to form lasting protection for the substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of ceramic coatings, and in particular to an aerogel ceramic coating and a preparation process thereof. Background Art

[0002] With the rapid development of urbanization in China, the possibility of fires is increasing due to the dense urban population, high-rise residential buildings and the widespread use of new building materials, especially decorative materials. Fire accidents have become one of the main civil engineering disasters. Therefore, strengthening the research and application of functional fireproof materials has become a key topic in the theoretical and engineering circles.

[0003] Fire retardant coating is a kind of fireproof material, which is often used to coat the surface of combustible substrates to reduce the flammability of the coated material surface and block the rapid spread of fire, or coated on the surface of structural materials to improve the fire resistance limit of components. However, in some practical applications, there are certain drawbacks. For example, inorganic fireproof materials based on water glass have water resistance problems, and non-expanding fireproof coatings based on cement have problems such as thick coating, low bonding strength, and easy to fall off in the later stage. Organic fireproof materials are expensive and have certain toxicity, which can easily pollute the environment and endanger human health.

[0004] In recent years, ceramic coatings have attracted much attention as an inorganic water-based coating. They are usually made of nano-inorganic compounds as film-forming substances, water as solvent, and other fillers, additives, etc. When ceramic coatings are cured, as the water evaporates, the polymer particles squeeze each other and eventually cross-link to form a ceramic phase coating. Ceramic coatings have the advantages of high wear resistance, high corrosion resistance, high temperature resistance, and high chemical resistance. With the widespread application of ceramic coatings in the construction field, the performance requirements of ceramic coatings are also increasing.

[0005] In order to improve the thermal insulation and fireproof performance of ceramic coatings, some studies have used aerogel as an additive to prepare ceramic coatings. Aerogel is a solid material with excellent thermal insulation performance, with special microstructures such as high specific surface area, nanoscale pores, and low density. However, it is precisely because of these structural characteristics that aerogel coatings are difficult to develop: the nanoporous structure is easily blocked by liquid media or nanoscale components, resulting in structural destruction, low density and porosity make it very fragile, and the mechanical properties are insufficient. These shortcomings make the aerogel coating system unstable, and the thermal insulation and mechanical properties of the formed coating cannot be improved ideally. Summary of the invention

[0006] In order to solve the problems existing in the above-mentioned prior art, such as unstable aerogel material structure resulting in unstable aerogel ceramic coating system, poor thermal insulation and fire resistance of the coating, insufficient mechanical properties, etc., the present invention provides an aerogel ceramic coating and a preparation process thereof.

[0007] An aerogel ceramic coating comprises the following components by mass percentage: 21-32% alkoxysilane, 15-25% orthosilicate, 3.8-5.5% modified polyimide aerogel, 0.2-0.5% catalyst, 12-20% additive and 25-40% deionized water; wherein the modified polyimide aerogel is prepared by polymerizing a diamine having a structure of formula I and diaminodiphenyl ether as diamine mixed monomers with dianhydride, and mixing with perfluoropolyether siloxane;

[0008] ,

[0009] In formula I, R1 is a C2-3 alkylene group, and R2, R3, R4, and R5 are each independently a C2-5 alkyl group, a C1-5 fluorinated alkyl group, or a phenyl group.

[0010] In some embodiments of the present invention, the alkoxysilane is at least one of methyltrimethoxysilane, phenyltrimethoxysilane, dimethyldimethoxysilane, and methylphenyldimethoxysilane.

[0011] In some embodiments of the present invention, the orthosilicate is at least one of methyl orthosilicate and ethyl orthosilicate.

[0012] In some embodiments of the present invention, the method for preparing the modified polyimide aerogel comprises the following steps:

[0013] S1: In an inert gas atmosphere, a diamine mixed monomer and a dianhydride monomer are added to an organic solvent in sequence until they are completely dissolved, a fluorinated silicone and a polyphenylmethane polyamine are dissolved in the organic solvent and added to the above solution, and stirred to increase the viscosity of the solution;

[0014] S2: adding anhydride and alkaline catalyst to the mucus formed in S1 for imidization, pouring it out after 7-10 hours to make it gel, aging it at room temperature for 20-24 hours, replacing the organic solvent, and vacuum drying to obtain the modified polyimide aerogel.

[0015] In some embodiments of the present invention, the inventors have found that when the molar ratio of the diamine having the structure of Formula I in the diamine monomer mixed system is higher than 1:1, the porous structure of the modified polyimide aerogel finally prepared will break through the nanoscale pore size and tend to become larger, which is not conducive to the modified polyimide aerogel maintaining the pore structure and specific surface area in the ceramic coating, and its curing shrinkage rate will also increase. Therefore, the diamine mixed monomer is obtained by mixing the diamine having the structure of Formula I with diaminodiphenyl ether at a molar ratio of 0.5-1:1.

[0016] The addition of diamine having the structure of formula I makes the polyimide aerogel structure have a thicker strand structure and a smaller average pore size; the presence of side chains such as alkyl, fluorinated alkyl and phenyl groups prevents the close stacking of polymer molecular chains, reduces its shrinkage rate to a certain extent, and increases the stability of the aerogel pore structure.

[0017] In some embodiments of the present invention, the dianhydride monomer is at least one of aromatic dianhydrides, and specific examples thereof include biphenyl dianhydride, pyrophthalic anhydride, hexafluoro dianhydride, and the like.

[0018] In some embodiments of the present invention, the molar ratio of the diamine mixed monomer to the dianhydride monomer is 1:1.5-2.

[0019] In some embodiments of the present invention, the organic solvent is at least one of N-methylpyrrolidone, N,N-dimethylformamide, dimethyl sulfoxide, and tetrahydrofuran.

[0020] In some embodiments of the present invention, in the process of preparing the polyimide aerogel, the added fluorinated siloxane can be specifically selected from but not limited to: perfluorodecyltriethoxysilane (product number: SCA-F17C10E), dodecafluoroheptylpropylmethyldimethoxysilane (product number: SCA-F17C10T), dodecafluoroheptylpropyltrimethoxysilane (SCA-F17C10M), trifluoropropylmethyldimethoxysilane (product number: SCA-F3C3T), trifluoropropyltrimethoxysilane (SCA-F3C3M), perfluorooctyltriethoxysilane (SCA-F13C8E), perfluorooctyltrimethoxysilane (SCA-F13C8M), etc. of Nanjing Nengde New Materials; the added amount is 10-20% of the mass of the diamine mixed monomer.

[0021] The inventors found through experimental comparison that an appropriate amount of fluorinated silicone can squeeze the polyimide network structure to form a tighter pore wall structure, effectively reducing the effect of solvent surface tension and capillary action on aerogel shrinkage during coating curing, so that the aerogel maintains a lower density, shrinkage rate and higher porosity. If it is less than 10%, the shrinkage rate of polyimide aerogel cannot be effectively reduced, and the structural stability of the modified polyimide aerogel is poor; if it is greater than 20%, since fluorinated silicone will form particles in the pores, compressing the polyimide nano-network structure will greatly increase the pore size, increase the possibility of nano-scale components in the ceramic coating system entering the aerogel pores, thereby reducing the thermal insulation of the ceramic coating.

[0022] When preparing the modified polyimide aerogel, the added polyphenylmethane polyamine is a mixture containing 4,4'-diaminodiphenylmethane, 2,4'-diaminodiphenylmethane, 2,2'-diaminodiphenylmethane and polyphenylmethane polyamine, which serves as a crosslinking agent, and the addition amount accounts for 1.5-2% of the total mass of the diamine mixed monomer and the dianhydride monomer, so as to promote the crosslinking reaction of the oligomers in the system and the entanglement of the molecular chains, thereby forming a nanofibrous network structure.

[0023] In some embodiments of the present invention, the additives in the aerogel ceramic coating include leveling agents, dispersing agents, fillers, etc. The leveling agent may be, but not limited to, TEGO-375, TEGO-490, TEGO-492, etc., the dispersing agent may be, but not limited to, BYK108, BYK118, BYK191, BYK190, BYK101N, ANTI-TERRA-205, etc., and the filler may be, but not limited to, nano titanium dioxide, nano silicon dioxide, mica, talc, kaolin, etc.

[0024] A preparation process of the aerogel ceramic coating comprises the following steps: in a uniaxial multifunctional paint mixing kettle, alkoxysilane, orthosilicate and deionized water are first added into one of the mixing kettles according to metered dosage, and then a catalyst is slowly added to form a system A; in another mixing kettle, modified polyimide aerogel, an auxiliary agent and deionized water are added and mixed according to metered dosage to form a system B, the solution systems in the two mixing kettles are mixed and stirred, and dust is removed while stirring to obtain the aerogel ceramic coating.

[0025] In some embodiments of the present invention, the single-axis multifunctional mixing kettle used to prepare the aerogel ceramic coating is composed of at least two mixing kettles and a rotating shaft, and the rotation speed in each mixing kettle remains consistent; and the filler mixing kettle also has a dust reduction function.

[0026] Beneficial effect: Compared with the prior art, the aerogel ceramic coating prepared by the present invention uses a self-made modified polyimide aerogel as one of the fillers. The modified polyimide aerogel is prepared by mixing a terminal amino disiloxane containing a side group with diaminodiphenyl ether as a diamine mixed monomer, amidating and polymerizing with an aromatic dianhydride monomer, and then crosslinking itself under the action of polyphenylmethane polyamine while mixing with a fluorinated siloxane:

[0027] 1. Due to the stability of the modified polyimide aerogel structure and the alkyl, fluoroalkyl, phenyl and other groups contained in its internal structure, the hardness, scrub resistance and acid and alkali resistance of the aerogel ceramic coating prepared by the present invention are greatly improved;

[0028] 2. The addition of the modified polyimide aerogel effectively alleviates the disadvantage of the coating's weak impact resistance due to its strong rigidity. This is because the modified polyimide aerogel contains flexible ether bonds and a high porosity, so that when the coating is impacted, the porous structure can quickly disperse the force to the surroundings, and there will be no cracking or peeling;

[0029] 3. The stable porous structure of the modified polyimide aerogel greatly reduces the thermal conductivity of the aerogel ceramic coating, and has a good protective effect on substrates with thermal insulation requirements;

[0030] 4. The mixing preparation of the aerogel ceramic coating is carried out in a self-developed single-axis multifunctional paint mixing kettle, which adopts an efficient feeding-paint mixing-dust reduction integrated process production route to achieve stable and rapid production of ceramic coatings. DETAILED DESCRIPTION

[0031] The present invention is described in further detail below in conjunction with examples. It should be noted that the following embodiments and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various improvements within the concept of the present invention may be carried out without departing from the gist or scope of the present invention.

[0032] The following is an exemplary description of the preparation process of the modified polyimide aerogel used in the embodiment:

[0033] Modified polyimide aerogel-1

[0034] S1: Under a nitrogen atmosphere, 3.0 mmol (0.924 g) of a diamine monomer having a structure of formula I-1 and 6.0 mmol (2.0025 g) of 4,4-diaminodiphenyl ether were added to N-methylpyrrolidone (NMP) until completely dissolved, and then 13.5 mmol (3.9720 g) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added and mechanically stirred until completely dissolved, and then 0.2927 g of trifluoropropyltrimethoxysilane (SCA-F3C3M) and 0.1035 g of polyphenylmethane polyamine were dissolved in NMP and added to the above solution, and stirred to increase the viscosity of the solution;

[0035]

[0036] S2: Add 10 ml of acetic anhydride and 5 ml of triethylamine to the mucus formed in S1 for imidization, pour it out after 7 hours to make it gel, age it at room temperature for 24 hours, replace the NMP with acetone and ethanol, and then vacuum dry it to obtain the modified polyimide aerogel-1.

[0037] Modified polyimide aerogel-2

[0038] S1: Under a nitrogen atmosphere, 4.5 mmol (1.4445 g) of a diamine monomer having a structure of formula I-2 and 6.0 mmol (2.0025 g) of 4,4-diaminodiphenyl ether were added to N-methylpyrrolidone (NMP) until completely dissolved, and then 18.9 mmol (5.5608 g) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added and mechanically stirred until completely dissolved, and then 0.5171 g of dodecafluoroheptylpropylmethyldimethoxysilane (SCA-F17C10T) and 0.1621 g of polyphenylmethane polyamine were dissolved in NMP and added to the above solution, and stirred to increase the viscosity of the solution;

[0039]

[0040] S2: 10 ml of acetic anhydride and 5 ml of triethylamine were added to the mucus formed by S1 for imidization, and the mixture was poured out after 8 hours to make it gel, and aged at room temperature for 24 hours. After solvent replacement of NMP with acetone and ethanol, the mixture was vacuum dried to obtain the modified polyimide aerogel-2.

[0041] Modified polyimide aerogel-3

[0042] S1: Under a nitrogen atmosphere, 6.0 mmol (1.9320 g) of a diamine monomer having a structure of formula I-3 and 6.0 mmol (2.0025 g) of 4,4-diaminodiphenyl ether were added to N-methylpyrrolidone (NMP) until they were completely dissolved, and then 24.0 mmol (7.0613 g) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added and mechanically stirred until they were completely dissolved, and then 0.7869 g of perfluorooctyltrimethoxysilane (SCA-F13C8M) and 0.2199 g of polyphenylmethane polyamine were dissolved in NMP and added to the above solution, and stirred to increase the viscosity of the solution;

[0043]

[0044] S2: 15 ml of acetic anhydride and 8 ml of triethylamine were added to the mucus formed in S1 for imidization, and the mixture was poured out after 8 hours to make it gel, and aged at room temperature for 24 hours. After solvent replacement of NMP with acetone and ethanol, the mixture was vacuum dried to obtain the modified polyimide aerogel-3.

[0045] Modified polyimide aerogel-4

[0046] S1: Under a nitrogen atmosphere, 6.0 mmol (2.2320 g) of a diamine monomer having a structure of formula I-4 and 6.0 mmol (2.0025 g) of 4,4-diaminodiphenyl ether were added to N-methylpyrrolidone (NMP) until they were completely dissolved, and then 24.0 mmol (7.0613 g) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added and mechanically stirred until they were completely dissolved, and then 0.8649 g of perfluorodecyltriethoxysilane (SCA-F17C10E) and 0.2277 g of polyphenylmethane polyamine were dissolved in NMP and added to the above solution, and stirred to increase the viscosity of the solution;

[0047]

[0048] S2: 15 ml of acetic anhydride and 8 ml of triethylamine were added to the mucus formed in S1 for imidization, and the mixture was poured out after 10 hours to make it gel, and aged at room temperature for 24 hours. After solvent replacement of NMP with acetone and ethanol, the mixture was vacuum dried to obtain the modified polyimide aerogel-4.

[0049] Modified polyimide aerogel-5

[0050] S1: Under a nitrogen atmosphere, 6.0 mmol (2.9520 g) of a diamine monomer having a structure of formula I-5 and 6.0 mmol (2.0025 g) of 4,4-diaminodiphenyl ether were added to N-methylpyrrolidone (NMP) until they were completely dissolved, and then 24.0 mmol (7.0613 g) of 3,3',4,4'-biphenyltetracarboxylic dianhydride was added and mechanically stirred until they were completely dissolved, and then 0.9909 g of trifluoropropylmethyldimethoxysilane (SCA-F3C3T) and 0.2403 g of polyphenylmethane polyamine were dissolved in NMP and added to the above solution, and stirred to increase the viscosity of the solution;

[0051]

[0052] S2: Add 20 ml of acetic anhydride and 10 ml of triethylamine to the mucus formed in S1 for imidization, pour it out after 10 hours to make it gel, age it at room temperature for 24 hours, replace the NMP with acetone and ethanol, and then vacuum dry it to obtain the modified polyimide aerogel-5.

[0053] Modified polyimide aerogel-6

[0054] The preparation process is similar to that of the modified polyimide aerogel-1, except that the added amount of trifluoropropyltrimethoxysilane (SCA-F3C3M) is changed to 0.2341 g.

[0055] Modified polyimide aerogel-7

[0056] The preparation process is similar to that of the modified polyimide aerogel-5, except that the addition amount of the trifluoropropylmethyldimethoxysilane (SCA-F3C3T) is changed to 1.0900 g.

[0057] Modified polyimide aerogel-8

[0058] The preparation process is similar to that of modified polyimide aerogel-5, except that no fluorinated silicone is added.

[0059] The preparation process of the aerogel ceramic coating in the embodiment and the comparative example is as follows: in a uniaxial multifunctional paint mixing kettle, alkoxysilane, orthosilicate and deionized water are first added into one of the mixing kettles according to a metered amount, and then the catalyst is slowly added to form a system A; in another mixing kettle, the modified polyimide aerogel, additives and deionized water are added and mixed according to a metered amount to form a system B, and the solution systems in the two mixing kettles are mixed and stirred, and dust is removed while stirring to obtain the aerogel ceramic coating.

[0060] The raw materials and proportions used in the examples and comparative examples are shown in Tables 1-1 and 1-2:

[0061]

[0062]

[0063] The aerogel ceramic coatings obtained in Examples 1-8 and Comparative Example 1 were applied on a metal substrate. The detailed construction steps are as follows:

[0064] 1. Select cast aluminum, cast iron, and cast magnesium substrates and clean the residues and foreign matter on the surface of the substrates;

[0065] 2. Use diamond sand to sandblast the substrate, and the roughness is controlled at 3.5-4.5μm;

[0066] 3. Use high-pressure water spray or compressed air to remove sandblasting particles and other foreign matter on the surface of the substrate;

[0067] 4. When the substrate is preheated to 40-60℃, use a common air spray gun to spray, and use wet spraying method to construct, the film thickness is 15-20μm;

[0068] 5. Place the sprayed workpiece in a 60-80℃ oven to dry for 5-10 minutes, then move it into a 200℃ oven for high-temperature curing for 20 minutes.

[0069] The products obtained in Examples 1-8 and Comparative Example 1 were constructed according to the above steps, and the performance test standards or methods of the coating films obtained under the same process parameters were as follows:

[0070] Hardness: According to the national standard GB / T 6739-86;

[0071] Acid and alkali resistance: Put the coating into 5% sulfuric acid and 5% sodium carbonate respectively, soak for 24 hours. If the coating peels off or loses gloss, it is considered qualified.

[0072] Washability: Tested using Shanghai Puyu JTX-II architectural coating washability tester;

[0073] Impact resistance: in accordance with GB / T1732-93 "Determination of impact resistance of paint film";

[0074] Thermal conductivity: tested using Shanghai Chengsi double-plate thermal conductivity tester CSI-3001;

[0075] Fire resistance: in accordance with the national standard "GB / T 5464-2010";

[0076] The test results are shown in Table 2:

[0077]

[0078] It can be seen from the data in Table 2 that the aerogel ceramic coating provided by the present invention has high hardness and good impact resistance, and has qualified acid and alkali resistance and scrubbability resistance; the thermal conductivity of the coating film formed by the aerogel ceramic coating is not less than 0.085 W / m•K, and the non-flammability grade reaches Class A.

[0079] The excellent properties of the aerogel ceramic coating described above are all related to the modified polyimide aerogel contained in the system: the porous and stable structure of the modified polyimide aerogel is conducive to improving the impact resistance of the coating and reducing its thermal conductivity, and the porous and stable structure of the modified polyimide aerogel is closely related to the fluorinated silicone (when the amount of fluorinated silicone added to the modified polyimide aerogel in Example 6 is too little, the pore structure inside the aerogel does not have many protective support structures, resulting in the poor impact resistance of the coating and increased thermal conductivity; when the amount of fluorinated silicone added to the modified polyimide aerogel in Example 7 is too much, the internal pores of the aerogel are easily blocked, and the thermal insulation of the coating is also reduced; when the modified polyimide aerogel in Example 8 does not add fluorinated silicone, the hardness, scrub resistance and impact resistance of the coating are all weakened); the modified polyimide aerogel and other components in the coating together give the coating a higher hardness, acid and alkali resistance and scrub resistance.

Claims

1. An aerogel ceramic coating, characterized in that: The invention comprises the following components by mass percentage: 21-32% alkoxysilane, 15-25% orthosilicate, 5.5% modified polyimide aerogel, 0.2-0.5% catalyst, 12-20% auxiliary agent and 25-40% deionized water; wherein the modified polyimide aerogel is prepared by polymerizing a diamine having a structure of formula I-5 and diaminodiphenyl ether as a diamine mixed monomer with a dianhydride monomer, and mixing with a fluorinated siloxane: ; The preparation method of the modified polyimide aerogel comprises the following steps: S1: In an inert gas atmosphere, a diamine mixed monomer and a dianhydride monomer are added to an organic solvent in sequence until they are completely dissolved, a fluorinated silicone and a polyphenylmethane polyamine are dissolved in the organic solvent and added to the above solution, and stirred to increase the viscosity of the solution; S2: adding anhydride and alkaline catalyst to the mucus formed in S1 for imidization, pouring it out after 7-10 hours to make it gel, aging it at room temperature for 20-24 hours, replacing the organic solvent, and vacuum drying to obtain the modified polyimide aerogel.

2. The aerogel ceramic coating according to claim 1, characterized in that: The alkoxysilane is at least one of methyltrimethoxysilane, phenyltrimethoxysilane, dimethyldimethoxysilane and methylphenyldimethoxysilane.

3. The aerogel ceramic coating according to claim 1, characterized in that: The orthosilicate is at least one of methyl orthosilicate and ethyl orthosilicate.

4. The aerogel ceramic coating according to claim 1, characterized in that: The diamine mixed monomer in S1 is obtained by mixing a diamine having a structure of formula I-5 and diaminodiphenyl ether in a molar ratio of 1:1; the dianhydride monomer is 3,3',4,4'-biphenyltetracarboxylic dianhydride.

5. The aerogel ceramic coating according to claim 1, characterized in that: The molar ratio of the diamine mixed monomer to the dianhydride monomer is 1:2; the molar amount of the fluorinated silicone is 41% of the molar amount of the diamine mixed monomer; and the mass of the polyphenylmethane polyamine is 2% of the total mass of the diamine mixed monomer and the dianhydride monomer.

6. The aerogel ceramic coating according to claim 1, characterized in that: The organic solvent in S1 is N-methylpyrrolidone.

7. The aerogel ceramic coating according to claim 1, characterized in that: The auxiliary agent comprises a leveling agent, a dispersing auxiliary agent and a filler.

8. A process for preparing the aerogel ceramic coating according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: in a uniaxial multifunctional paint mixing kettle, firstly adding alkoxysilane, orthosilicate and deionized water into one mixing kettle according to metered dosage, and then slowly adding a catalyst to form a system A; in another mixing kettle, adding and mixing modified polyimide aerogel, an auxiliary agent and deionized water according to metered dosage to form a system B, mixing and stirring the solution systems in the two mixing kettles, and removing dust while stirring to obtain the aerogel ceramic coating.

9. The process for preparing the aerogel ceramic coating according to claim 8, characterized in that: The single-shaft multifunctional paint mixing kettle is composed of at least two mixing kettles and a rotating shaft, and the rotation speed in each mixing kettle remains consistent.