A kind of multi-crosslinked polycarboxylate water reducer and preparation method thereof
Through the use of multi-component cross-linked polycarboxylate water-reducing agents, the problem of insufficient adaptability of cross-linked polycarboxylate water-reducing agents in complex concrete raw materials in the existing technology has been solved, and the workability and resistance of concrete have been significantly improved. Mud properties, improved glue dispersion and water film layer thickness, and increased concrete strength in low cement dosage systems.
Patent Information
- Application Number
- CN202311530750.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-11-16
AI Technical Summary
Existing cross-linked polycarboxylate superplasticizers have poor adaptability when faced with complex and changeable concrete raw materials, and are difficult to significantly improve the performance of concrete. Especially in systems with low cement dosage and low sand rate, they have poor workability. Inadequate clay resistance.
Using multi-component cross-linked polycarboxylate water-reducing agent, a variety of functional groups are introduced through the multi-component cross-linking agent to improve the molecular weight distribution and cross-linking configuration, enhance dispersion ability and adsorption strength, and combine with specific preparation methods and feeding methods to improve mud resistance. Performance and adaptability.
Significantly improves the workability and mud resistance of concrete, reduces sensitivity, improves the dispersion of glue particles and the thickness of the water film layer, enhances the adaptability to complex sand and gravel materials, and slightly improves in low cement dosage systems the strength of concrete.
Smart Images

Figure BDA0004553518190000081 
Figure BDA0004553518190000091 
Figure BDA0004553518190000093
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, in particular to the technical field of concrete admixtures, and specifically relates to a cross-linked polycarboxylate water-reducing agent and a preparation method thereof. Background Art
[0002] As concrete structures become larger, taller, and more complex, and as building materials develop toward low-carbon and green, the cement used in concrete has become finer, with a lower water-cement ratio, lower cement dosage, and more complex colloid components. The quality of various admixtures such as fly ash, mineral powder, and silica fume also varies greatly. At the same time, with the continuous depletion of high-quality sand and gravel resources in the region, inferior sand and gravel materials such as machine-made sand, washed sand, mountain sand, or artificial tailings sand with poor particle shape, poor gradation, multiple mineral components, and excessive mud content are gradually being used in large-scale projects. The development and changes of these concrete raw materials have resulted in poor workability of concrete prepared with ordinary polycarboxylate water-reducing agents, which has put forward higher requirements on the performance of polycarboxylate water-reducing agents.
[0003] The molecular structure of polycarboxylic acid is easy to adjust. Through molecular structure design, various ideal properties can be provided for polycarboxylic acid water-reducing agent to improve the performance of concrete mixture. Cross-linked polycarboxylic acid water-reducing agent adopts monomers with multiple polymerizable active ends. Without changing the existing materials and initiating polymerization system, the comb-type molecules are developed towards hyperbranched conformation. Hyperbranched cross-linked polycarboxylic acid water-reducing agent molecules have stronger adsorption and greater steric hindrance. They change the configuration of the main chain and side chain, increase the hydrophobic groups, increase the thickness of the formed water film layer, promote more uniform dispersion of cement particles, and thus improve the workability of fresh concrete. In addition, the cross-linking agent can play a role in the limited body network conformation in the molecular design of polycarboxylic acid water-reducing agent, significantly increase the molecular weight, significantly reduce the proportion of small molecular weight units, and improve the efficiency and effect of polyether.
[0004] Patent CN114736341A discloses a cross-linked polycarboxylic acid water-reducing agent and a preparation method thereof, wherein the cross-linked polycarboxylic acid water-reducing agent is prepared by free radical polymerization of hydroxyalkyl-terminated vinyl polyoxypropylene polyoxyethylene ether and trimethylolpropane polyoxyethylene polyoxypropylene ether triacrylate, and has the characteristics of high water reduction rate, high collapse retention, good encapsulation and excellent workability.
[0005] Patent CN113845627A discloses a cross-linked polycarboxylate water-reducing agent and its preparation method and use, wherein polycarboxylate polyglycol diester, acrylic acid and polyether monomers are mixed and copolymerized to obtain the cross-linked polycarboxylate water-reducing agent. By introducing polycarboxylate polyglycol diester monomers containing two double bonds to participate in the reaction, the single straight chain structure of the polycarboxylate water-reducing agent is transformed into a cross-linked network structure, thereby reducing its adsorption to powder in concrete, reducing the sensitivity of the polycarboxylate water-reducing agent, and improving the adaptability of the polycarboxylate water-reducing agent to concrete materials.
[0006] The cross-linked polycarboxylate water-reducing agents studied so far all use a single-component cross-linking agent for cross-linking. However, the adverse effect of simple molecular structure cross-linking on the adaptability of polycarboxylate water-reducing agents caused by complex harmful components is not obvious, and it is difficult to adapt to complex and changeable concrete raw materials, resulting in unsatisfactory actual application effects of this type of cross-linked polycarboxylate water-reducing agents. Summary of the invention
[0007] The present invention aims to solve the drawbacks of the prior art and provides a multi-crosslinked polycarboxylate water-reducing agent and a preparation method thereof, which has a simple and stable synthesis method, is environmentally friendly and efficient, and significantly improves the workability of concrete, has significant clay resistance, low sensitivity, and high adaptability.
[0008] A multi-component cross-linked polycarboxylate water-reducing agent, which is synthesized from the following raw material components by weight:
[0009] Polyether macromonomer: 440;
[0010] Multi-element cross-linking agent: 2.5 to 12 in total;
[0011] Unsaturated copolymer small monomer: 46~96;
[0012] Initiator: 2.5~4.5;
[0013] Reducing agent: 0.6~1.5;
[0014] Chain transfer agent: 1.6~4.5;
[0015] Water: 490-540;
[0016] The pH of the multi-crosslinked polycarboxylate water-reducing agent is 3-6, and the solid content is about 50%.
[0017] Furthermore, the reaction molar ratio of the unsaturated small monomer to the polyether macromonomer is (3.5-4.5):1.
[0018] Furthermore, the polyether macromonomer is one of allyl polyoxyethylene ether, methyl allyl polyoxyethylene ether, and isopentenyl polyoxyethylene ether, and has a molecular weight of 2400 to 3000.
[0019] Furthermore, the multi-crosslinking agent is a monomer having two or more polymerizable active ends, and is respectively composed of two or more of trimethylolpropane triacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, pentaerythritol triacrylate, ethylene glycol dimethacrylate, di(hydroxyethyl) phosphate, N,N'-vinylbisacrylamide, N,N'-methylenebisacrylamide, 1,6-hexanediol diacrylate, and tripropylene glycol diacrylate.
[0020] Furthermore, the unsaturated copolymerizable monomer is one or more of acrylic acid, methacrylic acid, maleic acid and maleic anhydride.
[0021] Furthermore, the initiator is one or more of hydrogen peroxide solution (30%), ammonium persulfate, potassium persulfate, and peracetic acid.
[0022] Furthermore, the reducing agent is one or more of L-ascorbic acid, bleaching agent, E51, ferrous sulfate, sodium bisulfite, sodium dithionite, and sodium thiosulfate.
[0023] Furthermore, the chain transfer agent is one or more of 2-mercaptoethanol, thioglycolic acid, 3-mercaptopropionic acid, 2-mercaptobutyric acid, and sodium hypophosphite.
[0024] The preparation method of the above-mentioned multi-crosslinked polycarboxylate water-reducing agent according to the present invention specifically comprises the following steps:
[0025] 1) Add polyether macromonomer, multi-element crosslinking agent and water into a reaction kettle, heat to 40-60°C, and stir thoroughly until completely dissolved;
[0026] 2) uniformly mixing the unsaturated copolymer monomer, the multi-element cross-linking agent and water to obtain material A;
[0027] 3) Mix the reducing agent, chain transfer agent and water evenly to prepare material B;
[0028] 4) Add the initiator into the reactor, stir for 3-5 minutes, then start to add material A and material B simultaneously, control the material A to be added within 120-210°C, control the material B to be added within 150-240°C, and continue to keep warm and stir for 30-60 minutes after the addition is completed;
[0029] 5) Add water to the reaction kettle to adjust the solid content to about 50%, stir evenly, and obtain a multi-crosslinked polycarboxylate water-reducing agent.
[0030] Furthermore, the multi-component cross-linking agent may be fed in the following ways according to the polymerization activity of each component:
[0031] 1) Add all into the reactor;
[0032] 2) Add all to material A;
[0033] 3) Take some amount and some types and add them into the reactor and material A respectively.
[0034] Compared with the prior art, the present invention has at least the following beneficial effects:
[0035] 1) The multi-crosslinked polycarboxylate water-reducing agent prepared by the present invention can increase the thickness of the water film layer coated on the adhesive particles, thereby significantly improving the workability of the prepared concrete.
[0036] 2) The present invention adopts a multi-crosslinking agent to crosslink and branch the polycarboxylic acid molecules, so that the polycarboxylic acid molecules obtain a wider molecular weight distribution and a richer molecular crosslinking configuration, so that the multi-crosslinked polycarboxylic acid can be more widely adapted to adhesives with different particle size distributions and sand and gravel with complex pore structures, greatly improving the adaptability of the polycarboxylic acid water reducer.
[0037] 3) The present invention adopts the idea of introducing a variety of beneficial functional groups through a multi-crosslinking agent, and can introduce unsaturated ester, phosphoric acid, and amide groups through a multi-crosslinking agent, thereby improving the dispersion ability and adsorption strength of the multi-crosslinked polycarboxylic acid, and can also effectively inhibit the harmful adsorption of components such as clay and montmorillonite, which can significantly improve the anti-mud performance of the polycarboxylic acid water reducer and reduce sensitivity.
[0038] 4) The multi-crosslinked polycarboxylate water-reducing agent prepared by the present invention has no adverse effect on the setting time, air content, strength and strength development of concrete. On the contrary, in concrete systems with low cement dosage, low sand ratio and poor workability, the multi-crosslinked polycarboxylate water-reducing agent can also slightly improve the strength of concrete.
[0039] 5) The preparation method of the present invention determines the feeding method according to the polymerization activity of the components in the multi-component cross-linking agent, thereby improving the utilization efficiency of the cross-linking agent.
[0040] 6) The preparation method of the present invention has the temperature of the entire synthesis process controlled at 40-60° C., has low energy consumption, is green and environmentally friendly, and the synthesis process is simple and efficient, has low requirements on production equipment, and is highly feasible. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0042] Example 1
[0043] 440g of isopentyl polyoxyethylene ether (molecular weight 2400), 1.5g of N,N'-methylenebisacrylamide, 7.3g of ethylene glycol dimethacrylate and 350g of water were added to a four-necked bottle reactor, heated to 50°C, and stirred to dissolve. 59g of methacrylic acid was mixed with 31g of water to obtain liquid A, and 1.2g of L-ascorbic acid and 2.8g of 2-mercaptoethanol were mixed with 86g of water to obtain liquid B. 4g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 150min, and liquid B was added dropwise for 180min. After the addition was completed, the mixture was stirred at the temperature for 60min, and then 33g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%.
[0044] Example 2
[0045] 440g of methyl allyl polyoxyethylene ether (molecular weight 2400), 3g of di(hydroxyethyl acrylate) phosphate and 350g of water were added to a four-necked bottle reactor, heated to 60°C, and stirred to dissolve. 50g of acrylic acid, 5g of polyethylene glycol diacrylate and 35g of water were mixed to obtain liquid A, and 1.2g of L-ascorbic acid and 2.4g of 2-mercaptoethanol were mixed with 86.4g of water to obtain liquid B. 4g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 150min, and liquid B was added dropwise for 180min. After the addition was completed, the mixture was stirred at the temperature for 60min, and then 27g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%.
[0046] Example 3
[0047] 440g of methyl allyl polyoxyethylene ether (molecular weight 2400), 1.5g of pentaerythritol triacrylate and 350g of water were added to a four-necked bottle reactor, heated to 60°C, and stirred to dissolve. 60g of methacrylic acid, 5.7g of polyethylene glycol dimethacrylate and 2g of N,N'-methylenebisacrylamide were shaken and mixed until completely dissolved, and then 22.3g of water was added and mixed evenly to obtain liquid A. 1g of E51 and 2.8g of 3-mercaptopropionic acid were mixed with 101.2g of water to obtain liquid B. 4g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 180min, and liquid B was added dropwise for 210min. After the addition was completed, the mixture was stirred at the temperature for 60min, and then 36g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%.
[0048] Example 4
[0049] 440g of isopentyl polyoxyethylene ether (molecular weight 3000) and 350g of water were added to a four-necked flask reactor, heated to 50°C, and stirred to dissolve. 47.5g of acrylic acid, 2.7g of diacrylate-1,6-hexanediol ester, and 5.4g of polyethylene glycol dimethacrylate were shaken and mixed until completely mixed and then 34.4g of water was added to obtain liquid A. 1g of L-ascorbic acid, 0.5g of ferrous sulfate solution (1%) and 88.5g of water were mixed to obtain liquid B. 4.5g of sodium hypophosphite was added to the reactor and stirred for 5min, then 4g of ammonium persulfate was added to the reactor and stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 180min, and liquid B was added dropwise for 210min. After the addition was completed, the mixture was stirred for 60min at a temperature, and then 28g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%.
[0050] Example 5
[0051] 440g of isopentyl polyoxyethylene ether (molecular weight 3000), 1.5g of trimethylolpropane triacrylate, 1.5g of tripropylene glycol diacrylate and 350g of water were added to a four-necked flask reactor, heated to 60°C, and stirred to dissolve. 60g of maleic anhydride, 1.7g of N,N'-vinyl bisacrylamide and 22.3g of water were mixed, heated in water, and shaken until completely dissolved to obtain liquid A. 1g of E51, 2.4g of 2-mercaptoethanol and 104.6g of water were mixed to obtain liquid B. 4.5g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 210min, and liquid B was added dropwise for 240min. After the addition was completed, it was stirred for 60min under heat preservation, and then 28g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%.
[0052] Comparative Example 1
[0053] 440g of methyl allyl polyoxyethylene ether (molecular weight 2400) and 350g of water were added to a four-necked bottle reactor, heated to 60°C, and stirred to dissolve. 50g of acrylic acid was mixed with 40g of water to obtain liquid A, and 1.2g of L-ascorbic acid and 2.4g of 2-mercaptoethanol were mixed with 86.4g of water to obtain liquid B. 4g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 180min, and liquid B was added dropwise for 210min. After the addition was completed, the mixture was stirred for 60min at a temperature of 50min, and then 15g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%. Compared with Example 2, no crosslinking agent component was added in this comparative example.
[0054] Comparative Example 2
[0055] 440g of methyl allyl polyoxyethylene ether (molecular weight 2400), 1.5g of pentaerythritol triacrylate and 350g of water were added to a four-necked bottle reactor, heated to 60°C, and stirred to dissolve. 60g of methacrylic acid was mixed with 30g of water to obtain liquid A, and 1g of E51 and 2.8g of 3-mercaptopropionic acid were mixed with 101.2g of water to obtain liquid B. 4g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 180min, and liquid B was added dropwise for 210min. After the addition was completed, the mixture was stirred for 60min at a temperature of 50min, and then 20g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%. Compared with Example 3, only a single crosslinking component was used in this comparative example.
[0056] Comparative Example 3
[0057] 440g of methyl allyl polyoxyethylene ether (molecular weight 2400), 1.5g of pentaerythritol triacrylate, 5.7g of polyethylene glycol dimethacrylate, 2g of N,N'-methylenebisacrylamide and 350g of water were added to a four-necked bottle reactor, heated to 60°C, and stirred to dissolve. 60g of methacrylic acid was mixed with 30g of water to obtain liquid A, and 1g of E51 and 2.8g of 3-mercaptopropionic acid were mixed with 101.2g of water to obtain liquid B. 4g of hydrogen peroxide solution (30%) was added to the reactor, stirred for 3min, and liquid A and liquid B were added dropwise at the same time. Liquid A was added dropwise for 180min, and liquid B was added dropwise for 210min. After the addition was completed, the mixture was stirred for 60min under heat preservation, and then 28g of water was added and stirred evenly to obtain a multi-crosslinked polycarboxylic acid water-reducing agent with a solid content of about 50%. Compared with Example 3, in this comparative example, the feeding method of each component in the multi-crosslinking agent is not distinguished, and the multi-crosslinking agent is all added to the bottom of the kettle at one time.
[0058] The polycarboxylate water-reducing agent samples synthesized in the examples and comparative examples were subjected to the anti-mud cement mortar fluidity test. The preparation of the test mortar was carried out with reference to GB / T 17671-2021 "Test Method for Cement Mortar Strength (ISO Method)", and the mortar mix ratio was slightly changed, the water-cement ratio was 0.35, and the mix ratio was shown in Table 1. The specific materials are: Huaxin Cement PO 42.5; China ISO standard sand; dry clay (powdered).
[0059] Table 1 Mortar mix ratio
[0060]
[0061] As for the mortar mix ratio mentioned above, the test was divided into two groups, 1# and 2#. The fluidity of the mortar was tested with a mortar expansion tube. In the 1# test, the initial fluidity of the mortar was controlled to be 350±20mm. In the 2# test, 2wt% (27g) of sand was replaced with clay. The test was carried out at the same admixture dosage, and the fluidity loss of the mortar before and after the addition of clay was compared.
[0062] The analysis of the test data of mortar fluidity in Table 2 shows that:
[0063] 1) Compared with the comparative example 1 without adding the cross-linking component, the fluidity loss of the other samples with adding the cross-linking component is lower than that of the comparative example 1, indicating that the addition of the cross-linking component can make the polycarboxylate water reducer obtain certain anti-mud and anti-sensitivity properties.
[0064] 2) Comparing Comparative Example 2 and Example 3, the fluidity loss of the polycarboxylate water-reducing agent mortar using a single component cross-linking system is much greater than that of Example 3 using a multi-component cross-linking system, indicating that the multi-component cross-linking polycarboxylate water-reducing agent has significant advantages in anti-mud and anti-sensitivity properties.
[0065] 3) Comparing Comparative Example 3 and Example 3, both are multi-crosslinked polycarboxylate water-reducing agents, but in Comparative Example 3, the feeding method of each component in the multi-crosslinking agent is not distinguished during the preparation process. The fluidity loss of the mortar is significantly greater than that of Example 3, indicating that in the preparation process of the multi-crosslinked polycarboxylate water-reducing agent, it is very important to distinguish the feeding method of each component in the multi-crosslinking agent, which can significantly improve the anti-mud and anti-sensitivity properties of the multi-crosslinked polycarboxylate water-reducing agent.
[0066] Table 2 Test data of mortar fluidity ratio
[0067]
[0068] The polycarboxylate water-reducing agent samples synthesized in the embodiment and the comparative example were compared for concrete application performance. The test method was tested in accordance with the national standards GB8076-2018 "Concrete Admixtures" and GB / T 50080-2016 "Test Methods for Performance of Ordinary Concrete Mixtures", and the initial slump, water seepage rate, emptying time of inverted slump cone, air content, setting time and 28d compressive strength of the cube were tested. The C25 concrete mix ratio is shown in Table 3, where the specific materials are: Huaxin cement, PO 42.5; mineral powder, S75 grade; fly ash, grade II; machine-made sand, Mx=2.4, MB=0.7; river sand, Mx=2.8, MB=1.1; crushed stone, particle size of 5-20 mm, continuous grading.
[0069] Table 3C25 concrete mix ratio
[0070]
[0071] Table 4 Concrete test data
[0072]
[0073]
[0074] The analysis of concrete test data in Table 4 shows that:
[0075] 1) Comparing Comparative Example 1 with the other samples, by observing the concrete state, adding a cross-linking agent can improve the workability of the mixed concrete to a certain extent, among which Examples 2 and 3 have the most obvious improvement on the workability of the concrete. In addition, data such as initial slump, water bleeding rate, and inverted slump cone emptying time also show such a trend. The water retention and fluidity of the concrete prepared with the uncross-linked polycarboxylate water-reducing agent are relatively poor, which shows that the cross-linked polycarboxylate water-reducing agent, especially the multi-cross-linked polycarboxylate water-reducing agent, can significantly improve the workability of the concrete mixture.
[0076] 2) Comparing Comparative Example 2 with Examples 1 to 5, the bleeding rate of Comparative Example 2 is significantly higher than that of the other examples, and the workability of the concrete state is far less than that of the other examples. This shows that compared with the single-component cross-linked polycarboxylate water-reducing agent, the multi-component cross-linked polycarboxylate water-reducing agent has a more significant advantage in improving workability and water retention.
[0077] 3) Comparing Comparative Example 3 with Example 3, both are multi-crosslinked polycarboxylate water-reducing agents, and the application effects in the concrete performance test are very good, but Example 3 performs better in terms of cohesiveness and water retention. This still shows that in the preparation process of the multi-crosslinked polycarboxylate water-reducing agent, it is very important to distinguish the feeding methods of the components in the multi-crosslinking agent.
[0078] 4) Comparing Examples 1 to 5 with Comparative Example 1, the multi-crosslinked polycarboxylate water-reducing agent has no adverse effect on the air content, setting time and strength of the concrete. On the contrary, in this concrete system with poor workability, the multi-crosslinked polycarboxylate water-reducing agent can improve the workability and also slightly increase the strength of the concrete.
[0079] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A multi-crosslinked polycarboxylate water-reducing agent, characterized in that: By weight, it is synthesized from the following raw material components: Polyether macromonomer: 440; Multi-crosslinking agent: 2.5 to 12 in total; Unsaturated copolymer small monomer: 46~96; Initiator: 2.5~4.5; Reducing agent: 0.6~1.5; Chain transfer agent: 1.6~4.5; Water: 490-540; The pH of the multi-crosslinked polycarboxylate water-reducing agent is 3-6, and the solid content is 50%; The polyether macromonomer is one of allyl polyoxyethylene ether, methyl allyl polyoxyethylene ether and isopentenyl polyoxyethylene ether, and has a molecular weight of 2400 to 3000; The multi-crosslinking agent is a monomer having two or more polymerizable active ends, and is respectively composed of two or more of trimethylolpropane triacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, pentaerythritol triacrylate, ethylene glycol dimethacrylate, di(hydroxyethyl) phosphate, N,N'-vinyl bisacrylamide, N,N'-methylene bisacrylamide, 1,6-hexanediol diacrylate, and tripropylene glycol diacrylate; The specific preparation method of the multi-crosslinked polycarboxylate water-reducing agent comprises the following steps: 1) Add polyether macromonomer, multi-element crosslinking agent and water into a reaction kettle, heat to 40-60°C, and stir thoroughly until completely dissolved; 2) uniformly mixing the unsaturated copolymer monomer, the multi-element cross-linking agent and water to obtain material A; 3) Mix the reducing agent, chain transfer agent and water evenly to prepare material B; 4) Add the initiator into the reactor, stir for 3-5 minutes, and then start to add material A and material B simultaneously. Control the addition of material A to be completed within 120-210 minutes, and control the addition of material B to be completed within 150-240 minutes. After the addition is completed, continue to keep warm and stir for 30-60 minutes; 5) Add water to the reaction kettle to adjust the solid content to 50%, stir evenly, and obtain a multi-crosslinked polycarboxylate water-reducing agent.
2. The multi-crosslinked polycarboxylate water-reducing agent according to claim 1, characterized in that: The reaction molar ratio of the unsaturated copolymer small monomer to the polyether macromonomer is 3.5-4.5:
1.
3. The multi-crosslinked polycarboxylate water-reducing agent according to claim 1, characterized in that: The unsaturated copolymerizable monomer is one or more of acrylic acid, methacrylic acid, maleic acid and maleic anhydride.
4. The multi-crosslinked polycarboxylate water-reducing agent according to claim 1, characterized in that: The initiator is one or more of 30% hydrogen peroxide solution, ammonium persulfate, potassium persulfate and peracetic acid.
5. The multi-crosslinked polycarboxylate water-reducing agent according to claim 1, characterized in that: The reducing agent is one or more of L-ascorbic acid, bleaching agent, E51, ferrous sulfate, sodium bisulfite, sodium dithionite, and sodium thiosulfate.
6. The multi-crosslinked polycarboxylate water-reducing agent according to claim 1, characterized in that: The chain transfer agent is one or more of 2-mercaptoethanol, thioglycolic acid, 3-mercaptopropionic acid, 2-mercaptobutyric acid, and sodium hypophosphite.
Citation Information
Patent Citations
Cross-linked type polycarboxylic acid water reducing agent as well as preparation method and application thereof
CN113845627A
Slow release slump retaining polycarboxylate water reducer and preparation thereof
CN102515618A