A method for selectively doping boron in solar cells
By using the hot wire chemical vapor deposition method to prepare a boron-doped amorphous silicon layer and performing oxygen-free boron diffusion in silicon solar cells, the problems of winding expansion, high laser energy and B2O3 by-product corrosion in the existing technology are solved, and high efficiency is achieved. The advanced boron diffusion process improves production efficiency and equipment life.
Patent Information
- Application Number
- CN202311207212.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-19
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-09-19
AI Technical Summary
The existing selectively doped boron diffusion process based on an oxygen boron source is prone to wraparound. It requires a large amount of chemical reagents to remove the boron wraparound layer on the non-diffused surface. The required laser energy is too high, which destroys the lattice structure of the silicon substrate. , and produce a large amount of B2O3 by-products to corrode quartz devices.
The boron-doped amorphous silicon layer is prepared by using hot wire chemical vapor deposition method, and laser selective heavy doping and oxygen-free boron diffusion are performed to replace the traditional boron-doped silicon oxide as the selective boron source, and the oxygen-free boron source is used for oxidation derivation. , avoiding the expansion and high-temperature annealing process, reducing the lattice damage of the laser to the silicon substrate and equipment maintenance costs.
It eliminates the need to consume a large amount of chemical reagents to remove the winding expansion layer, reduces the lattice damage of the laser to the silicon substrate, shortens the boron diffusion process time, improves production efficiency, extends the service life of the equipment, and avoids the impact of B2O3 by-products on quartz Corrosion of parts.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a method for selectively doping boron with solar cells. Background Art
[0002] Solar energy is a clean, efficient and inexhaustible new energy source, which has attracted widespread attention from researchers. Photovoltaic power generation has the advantages of safety, reliability, environmental protection and pollution-free. At present, due to the extremely rich reserves of silicon materials in the earth's crust and the excellent electrical and mechanical properties of silicon solar cells compared to other types of solar cells, silicon solar cells occupy an important position in the photovoltaic field.
[0003] In the preparation process of silicon solar cells, boron diffusion doping is the key to achieving high conversion efficiency of solar cells. Currently, the boron diffusion of mass-produced silicon solar cells adopts a uniform junction process with a low-concentration shallow junction structure. The low-concentration shallow junction structure will pose new challenges to the metal electrode slurry. Low-concentration doping can easily lead to poor contact resistance, high battery series resistance, and low fill factor FF. At the same time, shallow junction diffusion can easily increase the probability of electrode metal penetrating into the PN junction area, thereby reducing the conversion efficiency of the battery.
[0004] In order to obtain higher battery conversion efficiency, selective boron doping diffusion technology was born. Low-concentration shallow junctions are used in non-metallic contact areas, and high-concentration deep junctions are used in metal contact areas. While increasing the open circuit voltage and short-circuit current of the battery, the series resistance of the battery is reduced, and the fill factor of the battery is increased, thereby effectively improving the conversion efficiency of the battery.
[0005] At present, the selective doping boron diffusion still mainly uses the traditional CVD boron diffusion method to deposit the boron source, that is, the deposition method is to introduce an appropriate amount of boron chloride and oxygen into a high-temperature quartz furnace tube, and the boron chloride and oxygen react chemically to produce B2O3, and a layer of boron-doped silicon oxide (BSG) is generated on the silicon surface, and then the boron is diffused into the silicon surface to a certain depth through high-temperature nitrogen. After the boron source is deposited, the crystalline silicon cell is subjected to laser selective heavy doping treatment, and then placed in a high-temperature oxidation furnace tube for high-temperature push-in. While pushing the boron deeper into the silicon, the high temperature is used to repair the silicon substrate lattice damage caused by the laser treatment.
[0006] The above selective boron doping diffusion process has at least the following defects:
[0007] (1) The CVD reaction in the boron diffusion method is isotropic, that is, the boron source will be deposited on all exposed parts of the cell, and boron diffusion will occur at high temperature. In order to remove the wrap-around of the non-diffused surface, the non-diffused surface needs to be alkali-washed / acid-washed in the post-cleaning process and the silicon wafer needs to be etched to a certain thickness to achieve the purpose of removing the wrap-around. This de-wrapping process increases the consumption of chemicals and the cost of silicon wafers.
[0008] (2) During the high-temperature push-in process, the oxygen-boron source will destroy the pyramid structure of crystalline silicon due to high-temperature oxidation, increase the reflectivity of crystalline silicon, and reduce the ability of crystalline silicon to absorb light;
[0009] (3) The presence of oxygen-boron source will cause a large amount of B2O3 byproducts to be produced during the process, which is highly corrosive to quartz devices (such as diffusion cavity quartz tubes, silicon wafer carrier quartz boats, quartz furnace doors, etc.), reducing the service life (3 to 6 months);
[0010] (4) Boron-doped silicon oxide (BSG) is used as a selective boron source doping material. Since the solid solubility of boron in silicon dioxide is higher than that in silicon, very high laser energy is required to diffuse the boron in silicon dioxide into silicon. However, excessive laser energy will destroy the lattice structure of the silicon substrate. In order to repair the lattice structure damaged by laser, a long high-temperature repair process is required after the laser selective heavy doping treatment, which has low production efficiency, high energy consumption, and will reduce the service life of key components of the machine and increase maintenance costs.
[0011] The Chinese patent literature discloses "a method and device for selective laser doping of solar cells", and its announcement number is CN116598375A. The invention can shorten the overall diffusion time of the diffuser by selective laser doping in a liquid, i.e., a doping source solution, without adding a PSG / BSG deposition step, thereby improving production efficiency, saving doping sources, and saving production costs; the laser acts on the surface of the silicon wafer through the solution, which can further reduce the damage caused by the laser thermal effect. However, the process conditions of the invention are relatively harsh. On the one hand, the doping source solution must ensure a certain content of doping sources to provide sufficient doping sources for the laser SE. On the other hand, the doping solution needs to maintain rheological properties, ensure continuous circulation of the liquid, and maintain the uniformity and stability of the doping source concentration of the surface solution; in addition, the doping source solution also needs to have a certain transmittance through the wavelength band selected by the laser during doping to ensure that the laser effectively acts on the surface of the silicon wafer, and the controllability of the doping effect is poor. Summary of the invention
[0012] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide a method for selective boron doping diffusion of solar cells, which is used to solve the problems that the existing selective boron doping diffusion process based on oxygen boron source is prone to wrap-around diffusion, requires a large amount of chemical reagents to remove the boron wrap-around layer on the non-diffusion surface, the required laser energy is too high, which destroys the lattice structure of the silicon substrate and produces a large amount of B2O3 by-products to corrode quartz devices.
[0013] To achieve the above-mentioned purpose and other related purposes, the present invention is obtained by including the following technical solutions.
[0014] The present invention provides a method for selectively doping boron in a solar cell, comprising the following steps:
[0015] Step (1): placing a silicon wafer in a reaction chamber of a hot wire chemical vapor deposition device, evacuating the chamber, introducing silane, diborane and hydrogen, depositing a boron-doped amorphous silicon layer on one side of the silicon wafer, and exiting the chamber; the thickness of the boron-doped amorphous silicon layer is 10 to 30 nm;
[0016] Step (2): subjecting the surface of the silicon wafer treated in step (1) and deposited with the boron-doped amorphous silicon layer to a laser selective heavy doping treatment;
[0017] Step (3): placing the silicon wafer treated in step (2) in a boron diffusion furnace tube, evacuating the tube, and introducing nitrogen gas for oxygen-free boron diffusion;
[0018] Step (4): evacuate the boron diffusion furnace tube, purge with nitrogen, introduce oxygen, and perform oxidation and push-bonding on the silicon wafer treated in step (3) to complete the selective doping and diffusion of boron on the silicon wafer.
[0019] The present invention creatively uses a boron-doped amorphous silicon layer that is isotropic with silicon to replace the traditional boron-doped silicon oxide (BSG) as a selective boron source doping material. There is no difference in solid solubility between amorphous silicon and silicon. Driven by the boron concentration gradient, boron is easier to diffuse into silicon. Therefore, boron-doped amorphous silicon has a higher ion diffusion rate than boron-doped silicon oxide (BSG). On the one hand, it can diffuse ions to a greater depth using a lower laser power in laser selective heavy doping, thereby reducing the lattice damage of the laser to the silicon substrate, thereby reducing the repair time of subsequent high-temperature annealing, reducing the energy consumption of battery manufacturing, and reducing equipment costs; on the other hand, it can shorten the time of the boron diffusion process and improve mass production efficiency. The boron-doped amorphous silicon layer is prepared by hot wire chemical vapor deposition, and there is no wrap-around phenomenon. There is no need to consume a large amount of chemical reagents to etch and remove the wrap-around layer process, which reduces the amount of chemical reagents used and reduces the cost of the wet process. By using an oxygen-free boron source, no B2O3 byproducts are produced in the entire process, and no damage is caused to the quartz parts, reducing the equipment maintenance cost and extending the service life of the equipment.
[0020] Preferably, in step (2), the laser selective heavy doping process uses a green laser.
[0021] More preferably, the green laser has a pulse width of 500ps~2ns, and a scanning speed of 15000~35000m / s.
[0022] Preferably, in step (3), the pressure of oxygen-free boron diffusion is 300-500 mbar, the temperature is 900-930° C., and the time is 50-150 s.
[0023] Preferably, in step (4), the pressure of the oxidation push is 600-820 mbar, the temperature is 1000-1050° C., and the time is 40-80 min.
[0024] As described above, the method for selectively doping boron in solar cells of the present invention has the following beneficial effects:
[0025] (1) The boron-doped amorphous silicon layer is prepared by hot wire chemical vapor deposition, which will not cause the phenomenon of wrapping and expanding, and does not require the process of consuming a large amount of chemical reagents to etch and remove the wrapping and expanding layer, thereby reducing the amount of chemical reagents used and the cost of the wet process;
[0026] (2) The boron-doped amorphous silicon layer used as the selective boron source doping material has a low transmittance to green laser light. There is no need to perform high-temperature oxygen-free boron diffusion first. Laser selective heavy doping can be performed directly before entering the boron diffusion furnace tube, so that oxygen-free boron diffusion and oxidation push-in can be continuously produced without interrupting the boron diffusion process. There is no need to interrupt the boron diffusion process, and there will be no multiple exits and entry into the cavity, which will cause silicon wafer contamination. This is more conducive to mass production.
[0027] (3) Boron-doped amorphous silicon layer is used to replace the traditional boron-doped silicon oxide (BSG) as the selective boron source doping material. There is no difference in solid solubility between amorphous silicon and silicon. Driven by the boron concentration gradient, boron is easier to diffuse into silicon. Therefore, boron-doped amorphous silicon has a higher ion diffusion rate than boron-doped silicon oxide (BSG). On the one hand, it can diffuse ions to a greater depth using lower laser power during laser selective heavy doping, thereby reducing the laser lattice damage to the silicon substrate, thereby reducing the subsequent high-temperature annealing repair time, reducing the energy consumption of battery manufacturing, and reducing equipment costs; on the other hand, it can shorten the time of the boron diffusion process and improve mass production efficiency;
[0028] (4) By using oxygen-free boron source, no B2O3 by-products are produced in the entire process, which will not cause damage to quartz parts, reduce equipment maintenance costs, and extend the service life of the equipment. DETAILED DESCRIPTION
[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0030] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0031] In addition, it should be understood that one or more method steps mentioned in the present invention do not exclude the existence of other method steps before or after the combination step or the insertion of other method steps between these explicitly mentioned steps, unless otherwise specified; it should also be understood that the combination connection relationship between one or more devices / apparatuses mentioned in the present invention does not exclude the existence of other devices / apparatuses before or after the combination device / apparatus or the insertion of other devices / apparatuses between these explicitly mentioned two devices / apparatuses, unless otherwise specified. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0032] The active boron concentration of silicon wafers and the junction depth of PN junction in the following embodiments and comparative examples of the present application are tested using the ECV electrochemical test method commonly used in the industry.
[0033] In a specific embodiment, in step (1), the flow ratio of silane, diborane and hydrogen is 1: (2-2.85): (0.5-1).
[0034] In a more specific embodiment, in step (1), the flow rate of silane is 1300-1600 sccm; the flow rate of diborane is 3200-3700 sccm; and the flow rate of hydrogen is 800-1000 sccm.
[0035] In a specific embodiment, in step (1), the reaction pressure is 2-10 Pa.
[0036] In a specific embodiment, in step (1), the hot wire chemical vapor deposition equipment uses hot wire heating, and the temperature of the hot wire heating is 1750~1950℃.
[0037] In a specific embodiment, in step (2), the laser selective heavy doping treatment uses a green laser, the pulse width of the green laser is 500ps~2ns, and the scanning speed is 15000~35000m / s.
[0038] In a more specific embodiment, the power of the green laser is 10-20% lower than the power of the laser using conventional boron-doped silicon oxide as a source.
[0039] In a specific embodiment, in step (3), the flow rate of nitrogen is 2500-3000 sccm.
[0040] In a specific embodiment, in step (4), the flow rate of oxygen is 15000-20000 sccm.
[0041] Example 1
[0042] The present invention provides a method for selectively doping boron in a solar cell, comprising the following steps:
[0043] Step (1): placing a silicon wafer in a reaction chamber of a hot wire chemical vapor deposition device, evacuating the chamber, heating the chamber to 1950°C using a hot wire, introducing 1500 sccm of silane, 3700 sccm of diborane and 900 sccm of hydrogen to form a pressure of 3 Pa, depositing a 10 nm thick boron-doped amorphous silicon layer on one side of the silicon wafer, and exiting the chamber;
[0044] Step (2): subjecting the surface of the silicon wafer treated in step (1) and deposited with the boron-doped amorphous silicon layer to a laser selective heavy doping treatment; the laser selective doping treatment uses a green laser with a pulse width of 1 ns and a power of 25.5 W, which is 15% lower than the power of a conventional laser using boron-doped silicon oxide as a source, and a scanning speed of 15000 m / s;
[0045] Step (3): placing the silicon wafer treated in step (2) in a boron diffusion furnace tube, evacuating and purging, heating to 930°C, introducing 3000 sccm of nitrogen to form a pressure of 450 mbar, and performing oxygen-free boron diffusion for 100 seconds;
[0046] Step (4): evacuate the boron diffusion furnace tube, purge with nitrogen, introduce 20,000 sccm of oxygen to form a pressure of 800 mbar, raise the temperature to 1050° C., and perform oxidation on the silicon wafer treated in step (3) for 40 minutes to complete the selective doping of the silicon wafer with boron.
[0047] The boron expansion area of the silicon wafer obtained in this embodiment includes a non-laser heavily doped area and a laser heavily doped area, wherein the surface active boron concentration of the non-laser heavily doped area is 7.8E18 / cm 3 , with an active boron concentration of 1E17 / cm 3 The junction depth of the non-heavy laser doped region is 0.63 μm, and the surface active boron concentration of the heavily laser doped region is 1.2E19 / cm 3 , with an active boron concentration of 1E17 / cm 3 As the benchmark, the junction depth of the laser heavily doped area is 1.51μm.
[0048] Example 2
[0049] The present invention provides a method for selectively doping boron in a solar cell, comprising the following steps:
[0050] Step (1): placing a silicon wafer in a reaction chamber of a hot wire chemical vapor deposition device, evacuating the chamber, heating the chamber to 1950°C using a hot wire, introducing 1300 sccm of silane, 3500 sccm of diborane and 800 sccm of hydrogen to form a pressure of 2 Pa, depositing a 20 nm thick boron-doped amorphous silicon layer on one side of the silicon wafer, and exiting the chamber;
[0051] Step (2): subjecting the surface of the silicon wafer treated in step (1) and deposited with the boron-doped amorphous silicon layer to a laser selective heavy doping treatment; the laser selective doping treatment uses a green laser with a pulse width of 2 ns and a power of 24 W, which is 20% lower than the power of a conventional laser with boron-doped silicon oxide as the source, and a scanning speed of 25000 m / s;
[0052] Step (3): placing the silicon wafer treated in step (2) in a boron diffusion furnace tube, evacuating and purging, heating to 915°C, introducing 2500 sccm of nitrogen to form a pressure of 400 mbar, and performing oxygen-free boron diffusion for 50 seconds;
[0053] Step (4): evacuate the boron diffusion furnace tube, purge with nitrogen, introduce 15000 sccm of oxygen to form a pressure of 750 mbar, raise the temperature to 1025°C, and perform oxidation on the silicon wafer treated in step (3). The oxidation time is 60 minutes to complete the selective doping of boron on the silicon wafer.
[0054] The boron expansion area of the silicon wafer obtained in this embodiment includes a non-laser heavily doped area and a laser heavily doped area, wherein the surface active boron concentration of the non-laser heavily doped area is 7.7E18 / cm 3 , with an active boron concentration of 1E17 / cm 3 The junction depth of the non-heavy laser doped region is 0.62 μm, and the surface active boron concentration of the heavily laser doped region is 1.1E19 / cm 3 , with an active boron concentration of 1E17 / cm 3 As the benchmark, the junction depth of the laser heavily doped area is 1.47μm.
[0055] Example 3
[0056] The present invention provides a method for selectively doping boron in a solar cell, comprising the following steps:
[0057] Step (1): placing a silicon wafer in a reaction chamber of a hot wire chemical vapor deposition device, evacuating the chamber, heating the chamber to 1950° C. using a hot wire, introducing 1600 sccm of silane, 3200 sccm of diborane and 1000 sccm of hydrogen to form a pressure of 10 Pa, depositing a 30 nm thick boron-doped amorphous silicon layer on one side of the silicon wafer, and exiting the chamber;
[0058] Step (2): subjecting the surface of the silicon wafer treated in step (1) and deposited with the boron-doped amorphous silicon layer to a laser selective heavy doping treatment; the laser selective doping treatment uses a green laser with a pulse width of 500 ps and a power of 27 W, which is 10% lower than the power of a conventional laser with boron-doped silicon oxide as the source, and a scanning speed of 35000 m / s;
[0059] Step (3): placing the silicon wafer treated in step (2) in a boron diffusion furnace tube, evacuating and purging, heating to 900° C., introducing 2800 sccm of nitrogen to form a pressure of 500 mbar, and performing oxygen-free boron diffusion for 100 s;
[0060] Step (4): evacuate the boron diffusion furnace tube, purge with nitrogen, introduce 18000 sccm of oxygen to form a pressure of 820 mbar, raise the temperature to 1000°C, and perform oxidation on the silicon wafer treated in step (3). The oxidation time is 80 minutes to complete the selective doping of boron on the silicon wafer.
[0061] The boron expansion area of the silicon wafer obtained in this embodiment includes a non-laser heavily doped area and a laser heavily doped area, wherein the surface active boron concentration of the non-laser heavily doped area is 7.7E18 / cm 3 , with an active boron concentration of 1E17 / cm 3 The junction depth of the non-heavy laser doped region is 0.62 μm, and the surface active boron concentration of the heavily laser doped region is 1.02E19 / cm 3 , with an active boron concentration of 1E17 / cm 3 As the benchmark, the junction depth of the laser heavily doped area is 1.39μm.
[0062] Comparative Example 1
[0063] The comparative example of the present application provides a selective boron doping diffusion method, comprising the following steps:
[0064] Step (1): placing a silicon wafer in a boron diffusion furnace tube, evacuating the tube, introducing 2500 sccm nitrogen, 230 sccm boron trichloride and 800 sccm oxygen, heating to 890°C at a pressure of 150 Pa, and depositing a boron-doped silicon oxide layer with a thickness of 15-20 nm on the silicon wafer for 400 seconds;
[0065] Step (2): evacuate the boron diffusion furnace tube, purge with nitrogen, raise the temperature to 930°C, introduce 3000 sccm of nitrogen to form a pressure of 400 mbar, perform oxygen-free boron diffusion for 400 seconds, and exit the cavity;
[0066] Step (3): subjecting the silicon wafer processed in step (2) to laser selective heavy doping treatment; the laser for the laser selective doping treatment uses a green laser with a pulse width of 1 ns, a laser power of 30 W, and a scanning speed of 25000 m / s;
[0067] Step (4): Place the silicon wafer treated in step (3) back into the boron diffusion furnace tube, evacuate, purge with nitrogen, introduce 20,000 sccm of oxygen to form a pressure of 800 mbar, raise the temperature to 1050° C., and perform oxidation push-bonding on the silicon wafer treated in step (3) for 60 minutes to complete the selective boron doping diffusion of the silicon wafer.
[0068] The boron expansion area of the silicon wafer obtained in this comparative example includes a non-laser heavily doped area and a laser heavily doped area, wherein the surface active boron concentration of the non-laser heavily doped area is 8.1E18 / cm 3 With active boron concentration of 1E17 / cm 3 The junction depth of the non-heavy laser doped region is 0.72 μm, and the surface active boron concentration of the heavily laser doped region is 1.1E18 / cm 3 , with an active boron concentration of 1E17 / cm 3 As the benchmark, the junction depth of the laser heavily doped area is 1.48μm.
[0069] Comparative Example 2
[0070] The difference between Comparative Example 2 and Comparative Example 1 is that step (4) is different, and the rest of the process is exactly the same. Specifically:
[0071] Step (4): Place the silicon wafer treated in step (3) back into the boron diffusion furnace tube, evacuate, purge with nitrogen, introduce 20,000 sccm of oxygen to form a pressure of 800 mbar, raise the temperature to 1025° C., and perform oxidation push-bonding on the silicon wafer treated in step (3) for 80 minutes to complete the selective boron doping diffusion of the silicon wafer.
[0072] The boron expansion area of the silicon wafer obtained in this comparative example includes a non-laser heavily doped area and a laser heavily doped area, wherein the surface active boron concentration of the non-laser heavily doped area is 8.5E18 / cm 3 , with an active boron concentration of 1E17 / cm 3 The junction depth of the non-heavy laser doped region is 0.68 μm, and the surface active boron concentration of the heavily laser doped region is 1.2E19 / cm 3 , with an active boron concentration of 1E17 / cm 3 As a benchmark, the junction depth of the laser heavily doped area is 1.4μm.
[0073] Comparative Example 3
[0074] The difference between Comparative Example 3 and Comparative Example 1 is that step (4) is different, and the rest of the process is exactly the same. Specifically:
[0075] Step (4): The silicon wafer treated in step (3) is placed in the boron diffusion furnace tube again, evacuated, purged with nitrogen, and introduced with 20,000 sccm of oxygen to form a pressure of 800 mbar. The temperature is raised to 1000° C. The silicon wafer treated in step (3) is oxidized and pushed for 100 minutes to complete the selective boron doping diffusion of the silicon wafer.
[0076] The boron expansion area of the silicon wafer obtained in this comparative example includes a non-laser heavily doped area and a laser heavily doped area, wherein the surface active boron concentration of the non-laser heavily doped area is 8.9E18 / cm 3 , with an active boron concentration of 1E17 / cm 3 The junction depth of the non-heavy laser doped region is 0.61 μm, and the surface active boron concentration of the heavily laser doped region is 1.35E19 / cm 3 , with an active boron concentration of 1E17 / cm 3 As the benchmark, the junction depth of the laser heavily doped area is 1.31μm.
[0077] Comparative Examples 1 to 3 use traditional boron-doped silicon oxide (BSG) as the selective boron source doping material. Since boron-doped silicon oxide (BSG) has a high transmittance to green laser, it is impossible to directly use green laser to selectively dope boron in boron-doped silicon oxide. Therefore, it is necessary to first perform high-temperature oxygen-free boron diffusion, and then perform green laser selective boron diffusion. The process flow of the comparative example is relatively complicated, and the boron diffusion process needs to be interrupted, and the cavity needs to be exited and entered multiple times, which is easy to cause silicon wafer contamination and is not conducive to continuous production.
[0078] Embodiments 1 to 3 use a boron-doped amorphous silicon layer as a selective boron source doping material, and have a low transmittance to green laser light. There is no need to perform high-temperature oxygen-free boron diffusion first, and laser selective heavy doping treatment can be performed directly before entering the boron diffusion furnace tube, so that oxygen-free boron diffusion and oxidation push-junction can be produced continuously without interrupting the boron diffusion process, and there will be no multiple exits and entrances to the cavity, which will cause contamination of the silicon wafer, and is more conducive to mass production.
[0079] By comparing the experimental data of each embodiment with each comparative example, it can be seen that the technical solution of the present application can achieve a relatively lower boron doping concentration in the non-laser heavily doped area of the silicon wafer, which can reduce the Auger recombination caused by high-concentration boron doping in silicon without affecting the junction depth of the laser heavily doped area.
[0080] In addition, the power of the laser used in the laser selective heavy doping treatment process of Examples 1 to 3 is 10 to 20% lower than that of the comparative example, and there is no loss to the lattice structure of the silicon substrate. When the junction depth is close to the laser heavy doping area, no further high-temperature and long-term repair is required, and the energy consumption is lower, which improves the production efficiency. Examples 1 to 3 use an oxygen-free boron source. The entire process has no B2O3 by-products, and there is no problem of corrosion of the quartz furnace tube in Comparative Examples 1 to 3. Examples 1 to 3 use a boron-doped amorphous silicon layer to replace the boron-doped silicon oxide (BSG) of Comparative Examples 1 to 3 as a selective boron source doping material, which has a higher ion diffusion rate. The oxygen-free boron diffusion time is shortened by 350 to 250 seconds relative to the comparative example, greatly improving the production efficiency. After the boron diffusion oxidation and push-in of the silicon wafers obtained in Examples 1 to 3, since no boron expansion occurs, no further alkali washing is required to remove the expansion layer; after the boron diffusion oxidation and push-in of the silicon wafers obtained in Comparative Examples 1 to 3, a large amount of chemical reagents need to be consumed in the next step of solar cell preparation to remove the back-side silicon oxide expansion and polishing. Compared with the comparative document process, the technical solution of the present application shortens the alkali tank cleaning time and saves a large amount of chemicals due to the absence of boron expansion, and effectively avoids the high risk of fragmentation and low light utilization caused by excessive thinning of the silicon wafer due to de-expansion. In summary, the cell photoelectric conversion efficiency of the solar cell prepared by Examples 1 to 3 can be increased by 0.07 to 0.15% relative to Comparative Examples 1 to 3.
[0081] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for selectively doping boron in solar cells, characterized in that: The following steps are involved: Step (1): placing a silicon wafer in a reaction chamber of a hot wire chemical vapor deposition device, evacuating the chamber, introducing silane, diborane and hydrogen, depositing a boron-doped amorphous silicon layer on one side of the silicon wafer, and exiting the chamber; the thickness of the boron-doped amorphous silicon layer is 10-30 nm; the flow ratio of silane, diborane and hydrogen is 1: (2-2.85): (0.5-1); the flow rate of silane is 1300-1600 sccm; the flow rate of diborane is 3200-3700 sccm; the flow rate of hydrogen is 800-1000 sccm; the reaction pressure is 2-10 Pa; the hot wire chemical vapor deposition device adopts hot wire heating, and the hot wire heating temperature is 1750-1950°C; Step (2): subjecting the surface of the silicon wafer treated in step (1) and deposited with the boron-doped amorphous silicon layer to a laser selective heavy doping treatment; the laser selective heavy doping treatment uses a green laser; the green laser has a pulse width of 500 ps to 2 ns and a scanning speed of 15000 to 35000 m / s; Step (3): placing the silicon wafer treated in step (2) in a boron diffusion furnace tube, evacuating the tube, and introducing nitrogen gas for oxygen-free boron diffusion; the pressure of the oxygen-free boron diffusion is 300-500 mbar, the temperature is 900-930°C, and the time is 50-150 seconds; the flow rate of the nitrogen gas is 2500-3000 sccm; Step (4): evacuate the boron diffusion furnace tube, purge with nitrogen, introduce oxygen, and perform oxidation push-bonding on the silicon wafer treated in step (3) to complete the selective doping boron diffusion of the silicon wafer; the oxidation push-bonding pressure is 600-820 mbar, the temperature is 1000-1050°C, and the time is 40-80 min; the oxygen flow rate is 15000-20000 sccm.
Citation Information
Patent Citations
Selective laser doping method and device for solar cell
CN116598375A
Diffusion method for silicon wafer and photovoltaic silicon wafer
CN114497283A
Preparation method of solar cell emitter
CN116053333A