Preparation method of rare earth drier and rare earth drier

The preparation of rare earth drying agents through the reaction of isocaprylic acid with ammonia water and rare earth salts has solved the problems of high toxicity, high cost and poor stability of traditional drying agents, improved the stability and application range of products, and achieved reduced usage and cost Reduced effect.

CN117550965BActive Publication Date: 2024-11-12INNER MONGOLIA CAMO RARE EARTH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311534834.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-17
Publication Date
2024-11-12
Estimated Expiration
2043-11-17

AI Technical Summary

Technical Problem

Traditional drying agents such as lead soap, manganese soap and cobalt soap have high toxicity, high cost and shortage of resources. The volatility of low-carbon organic solvents leads to poor stability of rare earth drying agents, affecting storage and application.

Method used

Isooctanic acid is used as both a reactant and a solvent, reacting with ammonia water and soluble rare earth salts, and preparing isooctanic acid rare earth drying agent through the saponification process to avoid the introduction of low-carbon organic solvents, improve product stability and boiling point, and reduce storage difficulty.

Benefits of technology

It improves the stability and application range of rare earth drying agents, reduces the dosage, reduces the cost of coatings, and optimizes the production process through the recycling of ammonium chloride solids.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117550965B_ABST
    Figure CN117550965B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a rare earth drier and a rare earth drier prepared by the method for preparing the rare earth drier. The method for preparing the rare earth drier comprises the following steps: mixing a first isooctanoic acid as a reactant and a second isooctanoic acid as a solvent to obtain total isooctanoic acid; mixing ammonia water and total isooctanoic acid to obtain a first reaction liquid after sufficient reaction; mixing a soluble rare earth salt and the first reaction liquid to obtain a second reaction liquid after sufficient reaction, and the isooctanoic acid solution of isooctanoic acid rare earth obtained after separation of the second reaction liquid is the required rare earth drier. The method for preparing the rare earth drier uses isooctanoic acid as both a reactant and a solvent, and the rare earth drier finally prepared is an isooctanoic acid solution of isooctanoic acid rare earth, which avoids the introduction of a low-carbon organic solvent with a low boiling point and strong volatility, and the difficulty of preserving the isooctanoic acid solution of isooctanoic acid rare earth prepared is greatly reduced, and the scope of application is also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of drier preparation, in particular to a preparation method of a rare earth drier and the rare earth drier. Background Art

[0002] A drier is a substance that can accelerate the drying of the coating film and catalyzes the oxygen absorption and polymerization of the dry oil film. There are several explanations for the working principle of the drier: 1. The metal in the drier is reduced to a low atomic valence, and the antioxidant is oxidized, thereby accelerating the oxidation of the oil; 2. The drier can accelerate the destruction of the hydroperoxide bond formed by the oxygen absorption of the oil film, forming a stable oxygen bond, and the other unsaturated bonds of the oil are directly polymerized, reducing the amount of oxygen required; 3. The drier can absorb oxygen from the air and give it to the oil film, reducing the difficulty of the oil film absorbing oxygen. The mixed use of drier is more effective than using it alone. Traditional drier is the oxide, salt and organic acid soap of metals such as cobalt, manganese, lead, iron, zinc and calcium. There are many disadvantages in the traditional drier system, mainly reflected in the toxicity of lead soap causing environmental pollution, the dark color of manganese soap is not suitable for light-colored paint, and the cobalt soap is expensive and cobalt resources are scarce.

[0003] As a new type of drier, rare earth driers are gaining more and more attention due to their advantages such as low dosage and low toxicity. Specifically, rare earth driers are used in baking varnishes and have the high-temperature drying properties of iron driers. They can increase the cross-linking degree of the paint film to improve hardness and toughness, and can improve gloss and light retention. Rare earth driers have both surface drying and bottom drying properties, and have coordination properties, which can promote the actual drying of coatings such as alkyd resins. Therefore, rare earth driers can replace driers such as lead, manganese, zinc, and calcium, and their activity is higher than that of lead and zirconium. Their dosage is equivalent to 40%~80% of the dosage of traditional driers, which can reduce the cost of coatings.

[0004] The organic solution of rare earth isooctanoate is a common rare earth drier. Its preparation method is usually to mix isooctanoic acid and a low-carbon organic solvent, add a strong base and a rare earth salt in sequence, and finally obtain the organic solution of rare earth isooctanoate. However, the low-carbon organic solvent has a low boiling point, a low flash point and strong volatility. The volatilization of the low-carbon organic solvent to varying degrees causes the content of the cerium isooctanoate component to change to varying degrees, which will also cause unstable changes in the application of the product itself. In addition, because the product itself is volatile, it brings certain difficulties to storage. Summary of the invention

[0005] Based on this, it is necessary to provide a method for preparing a rare earth drier that can solve the above problems.

[0006] In addition, it is also necessary to provide a rare earth drier prepared by a preparation method of the rare earth drier.

[0007] A method for preparing a rare earth drier comprises the following steps:

[0008] Mixing a first isooctanoic acid as a reactant and a second isooctanoic acid as a solvent to obtain total isooctanoic acid, wherein the mass ratio of the first isooctanoic acid to the second isooctanoic acid is 50-90:100;

[0009] Mixing ammonia water and the total isooctanoic acid, and obtaining a first reaction solution after sufficient reaction, wherein the molar ratio of ammonia in the ammonia water to the total isooctanoic acid is 60-80:100;

[0010] The soluble rare earth salt and the first reaction liquid are mixed, and a second reaction liquid is obtained after sufficient reaction. The second reaction liquid is separated to obtain an isooctanoic acid solution of rare earth isooctanoate, and the isooctanoic acid solution of rare earth isooctanoate is the required rare earth drier, wherein the molar ratio of the first isooctanoic acid to the rare earth element in the soluble rare earth salt is 3:1.5~3.

[0011] In one embodiment, the operation of mixing the ammonia water and the total isooctanoic acid and fully reacting to obtain the first reaction liquid is: reacting the ammonia water and the total isooctanoic acid under stirring at a temperature of 20°C to 90°C for 0.5h to 1h to obtain the first reaction liquid.

[0012] In one embodiment, the rotation speed of the stirring state is 200 rpm to 500 rpm.

[0013] In one embodiment, the concentration of the ammonia water is 25 wt %.

[0014] In one embodiment, the operation of mixing the soluble rare earth salt and the first reaction liquid and obtaining the second reaction liquid after sufficient reaction is: reacting the soluble rare earth salt and the first reaction liquid under stirring at a temperature of 20° C. to 90° C. for 0.5 h to 1 h, and then adding hydrogen peroxide until the pH value of the reaction liquid is 4 to 5, to obtain the second reaction liquid.

[0015] In one embodiment, the rotation speed of the stirring state is 200 rpm to 500 rpm.

[0016] In one embodiment, the soluble rare earth salt is a cerium salt, a lanthanum salt or a neodymium salt.

[0017] In one embodiment, the soluble rare earth salt is anhydrous cerium trichloride.

[0018] In one embodiment, the operation of obtaining the isooctanoic acid solution of rare earth isooctanoate after separation of the second reaction liquid is: allowing the second reaction liquid to stand for stratification and retaining the upper oil phase, wherein the upper oil phase is the isooctanoic acid solution of rare earth isooctanoate.

[0019] A rare earth drier is prepared by the above-mentioned rare earth drier preparation method.

[0020] The preparation method of the rare earth drier uses isooctanoic acid as both a reactant and a solvent, and the rare earth drier finally prepared is an isooctanoic acid solution of rare earth isooctanoate, which avoids the introduction of low-carbon organic solvents with low boiling points and strong volatility. The storage difficulty of the prepared isooctanoic acid solution of rare earth isooctanoate is greatly reduced, the product stability is increased, and the boiling point of the isooctanoic acid solution of rare earth isooctanoate is relatively high, and the application range of the isooctanoic acid solution of rare earth isooctanoate is also improved.

[0021] In addition, the preparation method of the rare earth drier of the present invention uses ammonia water to saponify isooctanoic acid, so that the remaining water phase after the second reaction liquid is separated is an ammonium chloride aqueous solution, and the water phase can be evaporated and crystallized to obtain ammonium chloride solid, which can be used downstream. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] in:

[0024] Figure 1 The present invention is a flow chart of a method for preparing a rare earth drier according to one embodiment. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] like Figure 1 The preparation method of the rare earth drier according to one embodiment of the present invention comprises the following steps:

[0027] S10, mixing the first isooctanoic acid as a reactant and the second isooctanoic acid as a solvent to obtain total isooctanoic acid.

[0028] Wherein, the mass ratio of the first isooctanoic acid to the second isooctanoic acid is 50-90:100.

[0029] S20, mixing ammonia water and the total isooctanoic acid obtained in S10, and obtaining a first reaction solution after sufficient reaction.

[0030] The molar ratio of ammonia to total isooctanoic acid in the ammonia water is 60-80:100.

[0031] In this embodiment, the concentration of ammonia water is 25 wt %.

[0032] It should be pointed out that after ammonia water and total isooctanoic acid are mixed, a saponification reaction occurs.

[0033] Preferably, in this embodiment, the operation of mixing ammonia water and total isooctanoic acid and obtaining the first reaction liquid after sufficient reaction is: reacting ammonia water and total isooctanoic acid under stirring at a temperature of 20°C to 90°C for 0.5h to 1h to obtain the first reaction liquid.

[0034] Specifically, the rotation speed in the above stirring state is 200 rpm to 500 rpm.

[0035] It should be noted that, in the present embodiment, the reaction of aqueous ammonia and total isooctanoic acid at 20° C. to 90° C. is achieved by using an oil bath.

[0036] In other implementations, it can also be achieved in other ways.

[0037] S30, mixing the soluble rare earth salt and the first reaction liquid obtained in S20, and obtaining a second reaction liquid after sufficient reaction, and obtaining an isooctanoic acid solution of isooctanoic acid rare earth after separation of the second reaction liquid, and the isooctanoic acid solution of isooctanoic acid rare earth is the required rare earth drier.

[0038] The molar ratio of the first isooctanoic acid to the rare earth element in the soluble rare earth salt is 3:1.5-3.

[0039] Considering that the molar ratio of isooctanoic acid residue and rare earth element in isooctanoic acid rare earth is 3:1, in order to ensure that the first isooctanoic acid as a reactant fully reacts, the amount of soluble rare earth salt added is 1.5 to 3 times the theoretical value.

[0040] Preferably, in this embodiment, the soluble rare earth salt and the first reaction liquid are mixed, and the operation of obtaining the second reaction liquid after sufficient reaction is: the soluble rare earth salt and the first reaction liquid are reacted for 0.5h~1h under stirring at a temperature of 20°C~90°C, and then hydrogen peroxide is added until the pH value of the reaction liquid is 4~5 to obtain the second reaction liquid.

[0041] Specifically, the rotation speed in the above stirring state is 200 rpm to 500 rpm.

[0042] Preferably, in this embodiment, the soluble rare earth salt is a cerium salt, a lanthanum salt or a neodymium salt.

[0043] Preferably, in this embodiment, the soluble rare earth salt is an anhydrous product of a cerium salt, a lanthanum salt or a neodymium salt.

[0044] Specifically, in this embodiment, the soluble rare earth salt is cerium trichloride. At this time, the rare earth drier finally prepared is an isooctanoic acid solution of cerium isooctanoate.

[0045] In this embodiment, the cerium trichloride is 5N anhydrous cerium trichloride crystals.

[0046] Preferably, in this embodiment, the operation of mixing the soluble rare earth salt and the first reaction solution is: dissolving the soluble rare earth salt in water and then mixing the mixture with the first reaction solution.

[0047] In order to increase the concentration of the soluble rare earth salt, it is necessary to increase the concentration of the solution obtained by dissolving the soluble rare earth salt in water as much as possible.

[0048] Preferably, the operation of obtaining the isooctanoic acid solution of rare earth isooctanoate after separation of the second reaction liquid is: standing the second reaction liquid for stratification and retaining the upper oil phase, which is the isooctanoic acid solution of rare earth isooctanoate.

[0049] The preparation method of the rare earth drier uses isooctanoic acid as both a reactant and a solvent, and the rare earth drier finally prepared is an isooctanoic acid solution of rare earth isooctanoate, which avoids the introduction of low-carbon organic solvents with low boiling points and strong volatility. The storage difficulty of the prepared isooctanoic acid solution of rare earth isooctanoate is greatly reduced, the product stability is increased, and the boiling point of the isooctanoic acid solution of rare earth isooctanoate is relatively high, and the application range of the isooctanoic acid solution of rare earth isooctanoate is also improved.

[0050] In addition, the preparation method of the rare earth drier of the present invention uses ammonia water to saponify isooctanoic acid, so that the remaining water phase after the second reaction liquid is separated is an ammonium chloride aqueous solution, and the water phase can be evaporated and crystallized to obtain ammonium chloride solid, which can be used downstream.

[0051] The present invention also discloses an embodiment of a rare earth drier prepared by the preparation method of the rare earth drier.

[0052] The following are specific embodiments.

[0053] The cerium trichloride used in the embodiment is 5N anhydrous cerium trichloride crystals, the ammonia water is 25 wt % concentrated ammonia water purchased from Tianjin Xiangyu Chemical Industry and Trade Co., Ltd., and the isooctanoic acid is purchased from Tianjin Komiou Chemical Reagent Co., Ltd.

[0054] Example 1

[0055] 700 mL of the first isooctanoic acid as a reactant and 1000 mL of the second isooctanoic acid as a solvent were mixed to obtain total isooctanoic acid.

[0056] 370 mL of ammonia water and total isooctanoic acid were reacted under stirring conditions of 300 rpm and 55° C. (oil bath) for 1 h to obtain a first reaction solution.

[0057] 1216g of cerium trichloride was dissolved in 400mL of water and reacted with the first reaction liquid under stirring at a speed of 300rpm and a temperature of 55°C (oil bath) for 1h. After cooling to room temperature, hydrogen peroxide was added until the pH value of the reaction liquid reached 4.5 to obtain a second reaction liquid. The second reaction liquid was allowed to stand and stratified, and the upper oil phase was retained. The upper oil phase was the isooctanoic acid solution of cerium isooctanoate, and the isooctanoic acid solution of cerium isooctanoate was the required rare earth drier.

[0058] Example 2

[0059] 680 mL of the first isooctanoic acid as a reactant and 1000 mL of the second isooctanoic acid as a solvent were mixed to obtain total isooctanoic acid.

[0060] 500 mL of aqueous ammonia and total isooctanoic acid were reacted under stirring conditions of 300 rpm and 55° C. (oil bath) for 1 h to obtain a first reaction solution.

[0061] 1216g of cerium trichloride was dissolved in 400mL of water and reacted with the first reaction liquid under stirring at a speed of 300rpm and a temperature of 55°C (oil bath) for 1h. After cooling to room temperature, hydrogen peroxide was added until the pH value of the reaction liquid reached 4.5 to obtain a second reaction liquid. The second reaction liquid was allowed to stand and stratified, and the upper oil phase was retained. The upper oil phase was the isooctanoic acid solution of cerium isooctanoate, and the isooctanoic acid solution of cerium isooctanoate was the required rare earth drier.

[0062] Example 3

[0063] 660 mL of the first isooctanoic acid as a reactant and 1000 mL of the second isooctanoic acid as a solvent were mixed to obtain total isooctanoic acid.

[0064] 552 mL of ammonia water and total isooctanoic acid were reacted under stirring conditions of 300 rpm and 55° C. (oil bath) for 1 h to obtain a first reaction solution.

[0065] 1216g of cerium trichloride was dissolved in 400mL of water and reacted with the first reaction liquid under stirring at a speed of 300rpm and a temperature of 55°C (oil bath) for 1h. After cooling to room temperature, hydrogen peroxide was added until the pH value of the reaction liquid reached 4.5 to obtain a second reaction liquid. The second reaction liquid was allowed to stand and stratified, and the upper oil phase was retained. The upper oil phase was the isooctanoic acid solution of cerium isooctanoate, and the isooctanoic acid solution of cerium isooctanoate was the required rare earth drier.

[0066] Example 4

[0067] 640 mL of the first isooctanoic acid as a reactant and 1000 mL of the second isooctanoic acid as a solvent were mixed to obtain total isooctanoic acid.

[0068] 620 mL of aqueous ammonia and total isooctanoic acid were reacted under stirring conditions of 300 rpm and 55° C. (oil bath) for 1 h to obtain a first reaction solution.

[0069] 1216g of cerium trichloride was dissolved in 400mL of water and reacted with the first reaction liquid under stirring at a speed of 300rpm and a temperature of 55°C (oil bath) for 1h. After cooling to room temperature, hydrogen peroxide was added until the pH value of the reaction liquid reached 4.5 to obtain a second reaction liquid. The second reaction liquid was allowed to stand and stratified, and the upper oil phase was retained. The upper oil phase was the isooctanoic acid solution of cerium isooctanoate, and the isooctanoic acid solution of cerium isooctanoate was the required rare earth drier.

[0070] Example 5

[0071] 620 mL of the first isooctanoic acid as a reactant and 1000 mL of the second isooctanoic acid as a solvent were mixed to obtain total isooctanoic acid.

[0072] 746 mL of aqueous ammonia and total isooctanoic acid were reacted under stirring conditions of 300 rpm and 55° C. (oil bath) for 1 h to obtain a first reaction solution.

[0073] 1216g of cerium trichloride was dissolved in 400mL of water and reacted with the first reaction liquid under stirring at a speed of 300rpm and a temperature of 55°C (oil bath) for 1h. After cooling to room temperature, hydrogen peroxide was added until the pH value of the reaction liquid reached 4.5 to obtain a second reaction liquid. The second reaction liquid was allowed to stand and stratified, and the upper oil phase was retained. The upper oil phase was the isooctanoic acid solution of cerium isooctanoate, and the isooctanoic acid solution of cerium isooctanoate was the required rare earth drier.

[0074] The density, metal cerium content and water content of the rare earth drier (isooctanoic acid solution of cerium isooctanoate) prepared in Examples 1 to 4 were measured respectively. The test method is as follows. The results are shown in Table 1.

[0075] Density test: Measure the volume of a fixed solution, weigh it, and calculate the density of the solution.

[0076] Determination of metal content: The water phase is obtained by organic extraction principle, and then the EDTA titration method is used to calculate the metal cerium content.

[0077] Determination of moisture content: Use a moisture meter to measure.

[0078] Table 1

[0079]

[0080] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a rare earth drier, characterized in that: The steps include: Mixing a first isooctanoic acid as a reactant and a second isooctanoic acid as a solvent to obtain total isooctanoic acid, wherein the mass ratio of the first isooctanoic acid to the second isooctanoic acid is 50-90:100; The ammonia water and total isooctanoic acid are reacted for 0.5 h to 1 h under stirring at a temperature of 20° C. to 90° C. to obtain a first reaction solution, wherein the molar ratio of ammonia in the ammonia water to the total isooctanoic acid is 60 to 80:100; the rotation speed of the stirring state is 200 rpm to 500 rpm; The soluble rare earth salt and the first reaction liquid are reacted under stirring at a temperature of 20°C to 90°C for 0.5h to 1h, and then hydrogen peroxide is added until the pH value of the reaction liquid is 4 to 5 to obtain a second reaction liquid, and the second reaction liquid is allowed to stand for stratification, and an upper oil phase is retained, wherein the upper oil phase is the isooctanoic acid solution of the isooctanoic acid rare earth, and the isooctanoic acid solution of the isooctanoic acid rare earth is the required rare earth drier, wherein the molar ratio of the first isooctanoic acid to the rare earth element in the soluble rare earth salt is 3:1.5 to 3; The soluble rare earth salt is a cerium salt, a lanthanum salt or a neodymium salt.

2. The method for preparing the rare earth drier according to claim 1, characterized in that: The concentration of the ammonia water is 25wt%.

3. The method for preparing the rare earth drier according to claim 1, characterized in that: The rotation speed in the stirring state is 200 rpm to 500 rpm.

4. The method for preparing the rare earth drier according to claim 1, characterized in that: The soluble rare earth salt is anhydrous cerium trichloride.