A preparation method of metal molecular sieve catalyst and its product and application
By introducing nickel chloride into the ZSM-5 molecular sieve catalyst, the oxidative coupling reaction of methane and carbon monoxide can be efficiently catalyzed under mild conditions to generate acetic acid, which solves the problems of complex methane conversion steps and high energy consumption in the existing technology. Achieving efficient and low-cost catalytic effect.
Patent Information
- Application Number
- CN202311272160.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-09-28
AI Technical Summary
It is difficult for existing technologies to efficiently catalyze the conversion of methane into oxygenated chemicals, such as methanol, formic acid, and acetic acid, under mild conditions. In particular, the C-C coupling reaction steps are complex and energy-consuming, and traditional catalysts are expensive and toxic.
ZSM-5 molecular sieve catalyst is used to catalyze the oxidative coupling reaction of methane and carbon monoxide to generate acetic acid by mixing nickel chloride aqueous solution and ZSM-5 molecular sieve, ultrasonic treatment and roasting.
It achieves high selectivity and high yield of acetic acid generation, avoids high temperature energy consumption, simple catalyst preparation, low raw material cost, and is suitable for large-scale production.
Smart Images

Figure CN117654597B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fine chemical industry, and specifically relates to a preparation method of a metal molecular sieve catalyst and its product and application. Background Art
[0002] Methane is the main component of natural gas, shale gas and combustible ice. It is abundant in reserves and cheap, and is considered a potential alternative energy source to oil. In traditional industry, methane is indirectly converted into methanol by steam reforming with carbon dioxide into synthesis gas (CO+H2). However, this process has many reaction steps, high energy consumption (>450℃), and high investment requirements. In order to overcome these challenges, the direct conversion of methane into oxygenated chemicals such as methanol, formic acid and other high-value-added chemicals under mild conditions has important applications and strategic significance. Compared with C1 products, the conversion of methane into C2 products (acetic acid) involving CC coupling is more economical and more challenging.
[0003] The intermediate products (methanol, formic acid, etc.) of direct conversion of methane are more easily peroxidized to carbon dioxide. Therefore, the establishment of a catalytic reaction system is crucial for methane conversion. Acetic acid is an important chemical raw material and is widely used in the pharmaceutical, food and chemical industries. The traditional synthesis of acetic acid (i.e., the Monsanto process) uses expensive Rh-based catalysts, toxic CH3l and corrosive HI.
[0004] Constructing a highly active and highly selective methane / carbon monoxide oxidative coupling catalyst and reaction system is a technical problem to be solved. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and to briefly introduce some preferred embodiments.
[0006] As one aspect of the present invention, the present invention provides a method for preparing a metal molecular sieve catalyst, which comprises the following steps:
[0007] The ZSM-5 molecular sieve catalyst is placed in a container, vacuum degassed, a nickel chloride aqueous solution is added dropwise to the container, ultrasonically treated, vacuum degassed to remove moisture, dried, ground evenly, heated to 500-600° C. and calcined to obtain the metal molecular sieve catalyst.
[0008] As a preferred solution of the method for preparing the metal molecular sieve catalyst of the present invention: the concentration of the nickel chloride aqueous solution is 0.5-1 wt %.
[0009] As a preferred solution of the method for preparing the metal molecular sieve catalyst of the present invention: the content of ZSM-5 molecular sieve in the nickel chloride aqueous solution is 0.6-0.7 g / mL.
[0010] As a preferred embodiment of the method for preparing the metal molecular sieve catalyst of the present invention, the drying step is drying at 60 to 70° C. for 12 to 20 hours.
[0011] As a preferred solution of the method for preparing the metal molecular sieve catalyst of the present invention: the calcination is carried out by heating the temperature to 550° C. at a rate of 2° C. / min and calcining for 4 hours.
[0012] The present invention also provides the use of the metal molecular sieve catalyst in catalyzing the oxidative coupling of methane and carbon monoxide to produce acetic acid. 10 mg of the metal molecular sieve catalyst is dispersed in a 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, the autoclave is sealed, 2 MPa of methane and 1 MPa of carbon monoxide are introduced, heated to 80° C., and reacted for 3 hours to obtain acetic acid.
[0013] Beneficial effects of the present invention: The metal molecular sieve catalyst prepared by the present invention has high methane / carbon monoxide oxidative coupling selectivity and acetic acid yield. The raw material cost is low, the preparation method is simple, and the catalytic performance is high. These advantages make it possible to be mass-produced and applied in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0015] Figure 1 The performance diagram of catalysts with different metal loadings;
[0016] Figure 2 Utilization rate of H2O2 in catalysts with different metal loadings
[0017] Figure 3 The catalytic performance diagram for different CH4 / CO partial pressures;
[0018] Figure 4 This is the effect diagram of H2S and CO2 on the oxidative coupling performance of methane (ethane) and carbon monoxide;
[0019] Figure 5 The catalytic performance comparison chart of different carriers;
[0020] Figure 6 This is a comparison chart of the catalytic performance of different metals;
[0021] Figure 7 For in-situ EPR testing;
[0022] Figure 8High-magnification transmission electron microscopy (a) and spherical aberration-corrected transmission electron microscopy (b) of 0.5wt% Ni / ZSM-5. DETAILED DESCRIPTION
[0023] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with specific embodiments.
[0024] Embodiment 1:
[0025] Place 1 g of calcined ZSM-5 catalyst in a schlenk vial and degas under vacuum for 30 min. Dissolve 0.5 wt% (calculated as Ni) nickel chloride in 1.5 ml of deionized water and slowly inject it into a rubber-sealed schlenk vial with a needle syringe. Stir while adding dropwise to form a slurry. Ultrasonicate for 20 min and continue to degas under vacuum until most of the water is removed. Dry in an oven at 70°C for 12 h, grind evenly, heat to 550°C at 2°C / min and calcine for 4 h to obtain 0.5 wt% Ni / ZSM-5.
[0026] Methane / carbon monoxide oxidative coupling reaction:
[0027] 10 mg of catalyst (0.5 wt% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa methane and 1 MPa carbon monoxide, heated to 80 ° C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain methanol, formic acid, and acetic acid, such as Figure 1 As shown, the acetic acid yield is 7.96mmol / g / h±0.34, and the acetic acid selectivity is 78.24%±2.45. The H2O2 utilization rate is 63.4% ( Figure 2 ). Most of the carbon dioxide in the gas product is converted through carbon monoxide, so the pathway of methane peroxidation to carbon dioxide can be ignored.
[0028] The catalyst prepared by the present invention and the catalytic methane carbon monoxide oxidative coupling catalytic system have mild reaction conditions, avoid high temperature reaction, and avoid huge energy consumption. The catalyst preparation method is simple, the preparation time is short, the product acetic acid has high selectivity, and is conducive to large-scale production and practical application.
[0029] Study Example 1:
[0030] 1 g of calcined ZSM-5 catalyst was placed in a schlenk vial and vacuum degassed for 30 min. Xwt% (X = 0.1, 1, 2, 4; calculated as Ni) nickel chloride was dissolved in 1.5 ml of deionized water and slowly injected into a rubber-sealed schlenk vial with a syringe, and stirred while adding dropwise to form a homogenate. The mixture was ultrasonically treated for 20 min and vacuum degassed until most of the water was removed. The mixture was dried in an oven at 70°C for 12 h, ground evenly, and heated to 550°C at 2°C / min for 4 h to obtain Xwt% Ni / ZSM-5 (0.1wt% Ni / ZSM-5, 1wt% Ni / ZSM-5, 2wt% Ni / ZSM-5, and 4wt% Ni / ZSM-5, respectively).
[0031] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0032] 10 mg of catalyst (X% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa methane and 1 MPa carbon monoxide, heated to 80 ° C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain different contents of methanol, formic acid, and acetic acid, such as Figure 1 As shown, the H2O2 utilization rate is Figure 2 shown.
[0033] Study Example 2:
[0034] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0035] 10 mg of catalyst (0.5% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 3 MPa methane and 0 MPa carbon monoxide, heated to 80 ° C, and reacted for 3 h. The liquid product was found to contain only methanol and formic acid by NMR H spectroscopy, such as Figure 3 As shown, the methanol yield was 1.74 mmol / g / h±0.13, the formic acid yield was 5.74 mmol / g / h±0.37, and no acetic acid was produced.
[0036] Study Example 3:
[0037] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0038] 10 mg of the catalyst (0.5% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced with 0 MPa methane and 3 MPa carbon monoxide, heated to 80°C, and reacted for 3 hours. No liquid products such as methanol, formic acid, and acetic acid were found in the liquid product by H NMR spectrum detection.
[0039] Study 4:
[0040] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0041] 10 mg of catalyst (0.5% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa of methane, 1 MPa of carbon monoxide and 0.5 MPa of CO2, heated to 80 ° C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain methanol, formic acid, and acetic acid, such as Figure 4 As shown, the acetic acid yield is 7.81 mmol / g / h±0.41, the acetic acid selectivity in the liquid product is 76.27%±2.88, and the addition of CO2 has no obvious effect on the oxidative coupling of methane and carbon monoxide.
[0042] Study 5:
[0043] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0044] 10 mg of catalyst (0.5% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa methane, 1 MPa carbon monoxide and 5% (volume fraction) H2S, heated to 80°C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain methanol, formic acid, acetic acid, such as Figure 4 As shown, the acetic acid yield is 12.89mmol / g / h±0.64, and the acetic acid selectivity in the liquid product is 84.2%±3.14. The catalyst exhibits high sulfur resistance. H2S can be oxidized to S, SO2 and H2SO4. The presence of H2SO4 further promotes the selective oxidative coupling performance of methane.
[0045] Study 6:
[0046] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0047] 10 mg of catalyst (0.5% Ni / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa ethane and 1 MPa carbon monoxide, heated to 80 ° C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain methanol, formic acid, ethanol, acetic acid and propionic acid, such as Figure 4 As shown, the propionic acid yield is 11.76 mmol / g / h±0.59, and the acetic acid selectivity in the liquid product is 56.20%±2.74. The catalyst can be used for the selective oxidation of real biogas (natural gas).
[0048] Study Example 7:
[0049] Place 1 g of calcined commercial mordenite (MOR) or silica (SiO2) or alumina (Al2O3) in a schlenk vial and degas under vacuum for 30 min. Dissolve 0.5 wt% (calculated as Ni) nickel chloride in 1.5 ml of deionized water and slowly inject it into a rubber-sealed schlenk vial with a needle syringe while adding dropwise and stirring to form a homogenate. Ultrasonic treatment is performed for 20 min, and vacuum degassing is continued until most of the water is removed. The mixture is dried in an oven at 70°C for 12 h, ground evenly, heated to 550°C at 2°C / min and calcined for 4 h to obtain 0.5 wt% Ni / MOR, 0.5 wt% Ni / SiO2, and 0.5 wt% Ni / Al2O3, respectively.
[0050] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0051] 10 mg of catalyst (0.5 wt% Ni / ZSM-5 0.5 wt% Ni / MOR, 0.5 wt% Ni / SiO2, 0.5 wt% Ni / Al2O3) were dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa methane and 1 MPa carbon monoxide, heated to 80 ° C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain different contents of methanol, formic acid, and acetic acid, such as Figure 5 shown.
[0052] Study 8:
[0053] Place 1 g of calcined ZSM-5 catalyst in a schlenk vial and degas under vacuum for 30 min. Dissolve different metal salts (NiCl2, FeCl3, RhCl3, IrCl3, CuCl2, CoCl2) with a content of 0.5 wt% (calculated as metal) in 1.5 ml of deionized water, and slowly inject into a rubber-sealed schlenk vial with a needle syringe. Add dropwise while stirring to form a homogenate. Ultrasonicate for 20 min and continue to degas in vacuum until most of the water is removed. Dry in an oven at 70°C for 12 h, grind evenly, heat to 550°C at 2°C / min and calcine for 4 h to obtain M / ZSM-5 (M is Ni, Fe, Rh, Ir, Cu, Co, respectively).
[0054] Methane / Carbon Monoxide Oxidative Coupling Reaction Test
[0055] 10 mg of catalyst (0.5% M / ZSM-5) was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution, placed in a 100 mL autoclave, sealed, introduced 2 MPa methane and 1 MPa carbon monoxide, heated to 80 ° C, and reacted for 3 h. The liquid product was detected by H NMR spectrum and found to contain different contents of methanol, formic acid, and acetic acid, such as Figure 6 shown.
[0056] Study Example 9:
[0057] Through in situ EPR testing ( Figure 7 ), capturing the methyl radicals and hydroxyl radicals in the reaction, indicating that methane is first activated into methyl radicals, and then oxidative coupling reactions occur. H2O2 is split into hydroxyl radicals as the active oxygen species of the reaction, promoting the efficient progress of the reaction.
[0058] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. An application of a metal molecular sieve catalyst in catalyzing the oxidative coupling of methane and carbon monoxide to produce acetic acid, characterized in that: The preparation method of the metal molecular sieve catalyst is as follows: 1g of calcined ZSM-5 catalyst is placed in a bottle and vacuum degassed for 30 minutes; nickel chloride is dissolved in 1.5ml of deionized water to obtain a nickel chloride solution; wherein the content of Ni in the metal molecular sieve catalyst is 0.5wt%, the nickel chloride solution is slowly injected into the bottle sealed with a rubber seal, and stirred while adding dropwise to form a homogenate, and then ultrasonically treated for 20 minutes, and vacuum degassed continuously until most of the water is removed, and then dried in an oven at 70°C for 12 hours, ground evenly, and heated to 550°C at 2°C / min for 4 hours to obtain a metal molecular sieve catalyst 0.5wt% Ni / ZSM-5; 10 mg of metal molecular sieve catalyst 0.5 wt% Ni / ZSM-5 was dispersed in 0.1 mol / L hydrogen peroxide aqueous solution and placed in an autoclave. The autoclave was sealed, and 2 MPa of methane, 1 MPa of carbon monoxide and 5% by volume of H2S were introduced. The autoclave was heated to 80°C and reacted for 3 hours to obtain acetic acid.