A copper-based amorphous coating for ultra-high-speed blue-light laser cladding and a preparation method thereof

By adding specific elements to copper-based amorphous powder, using ultra-high-speed blue laser cladding technology and in-situ reactive heat treatment, the problems of structural instability and poor coating forming quality of amorphous powder under extreme operating conditions in the ocean are solved. A high-performance copper-based amorphous coating is achieved, which is suitable for long-term protection of marine engineering equipment.

CN117680673BActive Publication Date: 2024-10-01GUANGDONG INST OF NEW MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311783841.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-10-01
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

When used in extreme marine working conditions, existing amorphous powder materials have unstable structures and poor coating formation quality, and cannot meet the long-term protection needs of key moving parts of marine engineering equipment.

Method used

Develop a copper-based amorphous powder for ultra-high-speed blue laser cladding, containing 70-73% Cu, 10-14% Zr, 6-10% Ti, 5-9% Ni, 0.8-1.2% Si, 0.8-1.2 % B, through ultra-high-speed laser cladding technology and in-situ reaction heat treatment, a stable amorphous structure is formed to improve the wear resistance, corrosion resistance and anti-fouling performance of the coating.

Benefits of technology

The forming quality of the copper-based amorphous coating has been improved. The coating has no cracks and has excellent wear resistance, corrosion resistance and anti-fouling properties. It is suitable for surface protection of key moving parts serving in extreme marine working conditions and improves the equipment's durability. safety and service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117680673B_ABST
    Figure CN117680673B_ABST
Patent Text Reader

Abstract

The invention provides a copper-based amorphous powder for ultra-high-speed blue-light laser cladding and an application thereof. The copper-based amorphous powder for ultra-high-speed blue-light laser cladding comprises the following elemental components by mass percentage: 70-73% Cu, 10-14% Zr, 6-10% Ti, 5-9% Ni, 0.8-1.2% Si, and 0.8-1.2% B. The copper-based amorphous powder for ultra-high-speed blue-light laser cladding is composed of specific elements and content ranges, and the amorphous alloy powder has uniform particle size distribution, stable structure, excellent sphericity and fluidity, and the formed coating is metallurgically bonded to the substrate without cracks, and has excellent wear resistance, corrosion resistance and anti-fouling properties, high preparation efficiency, and small thermal impact on the substrate, and can be used for surface protection and remanufacturing of key moving parts serving in extreme marine working conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of surface engineering, and in particular to a copper-based amorphous powder for ultra-high-speed blue-light laser cladding and an application thereof. Background Art

[0002] Under extreme working conditions such as the ocean, the key moving parts of marine engineering equipment such as ship stern shafts and propellers suffer serious surface damage due to the coupling effects of wear, corrosion, and microbial fouling, which has a great impact on the safety and service life of equipment parts. Surface coating technology, as a means of surface protection for equipment parts, provides an important solution for high-performance impact-resistant, wear-resistant, and corrosion-resistant coatings in harsh marine conditions. Traditional coatings, thermal spraying, physical / chemical vapor deposition and other surface coating technologies are prone to failure and cannot play a protective role after long-term impact and mechanical action due to limited interface bonding strength, and cannot meet the long-term protection needs of key moving parts of marine engineering equipment. Laser cladding additive manufacturing technology has become an important technology for the preparation of wear-resistant and impact-resistant coatings due to its series of advantages such as controllable thickness, high metallurgical bonding strength and diverse materials.

[0003] Ultra-high-speed laser cladding technology is a new type of surface engineering technology. The overall manufacturing efficiency is 3-5 times higher than that of traditional laser cladding. It has the advantages of high efficiency, high performance, strong interface metallurgical bonding, green energy saving and environmental protection. It is expected to become a revolutionary alternative technology to traditional coating technology and provide an effective means for the preparation and application of surface protective coatings on key moving parts of marine engineering equipment.

[0004] Powder materials are the key foundation for the performance of ultra-high-speed laser cladding coatings. Currently, there is a lack of special powders for ultra-high-speed laser cladding coatings for extreme marine conditions. Amorphous alloys are different from traditional crystalline alloys. They are a type of solid material with unique structure and properties that is obtained by rapid cooling of alloy melts and has both metal and glass properties. Its internal atomic arrangement is long-range disordered like glass and has many unique properties. Due to its excellent performance and simple process, it is expected to become an important powder material raw material for surface protection of key moving parts of marine engineering equipment.

[0005] Chinese patent CN105525232B "A high entropy alloy amorphous powder for 3D printing and its preparation method" discloses a high entropy alloy amorphous powder for 3D printing, but the amorphous structure of the high entropy alloy amorphous powder is unstable and the coating forming quality is poor, and its performance still needs to be further improved.

[0006] Therefore, it is of great significance to develop a copper-based amorphous material for ultra-high-speed blue-light laser cladding with stable amorphous structure, good coating forming and excellent performance, and a preparation method thereof. Summary of the invention

[0007] In view of the fact that existing amorphous powder materials have unstable amorphous structure and poor coating forming quality, and their performance still needs to be further improved, the present invention provides a copper-based amorphous powder for ultra-high-speed blue light laser cladding and its application. The amorphous alloy powder has uniform particle size distribution, stable structure, excellent sphericity and fluidity, and the formed coating is metallurgically bonded to the substrate without cracks and has excellent wear resistance, corrosion resistance and anti-fouling properties. It has high preparation efficiency and little thermal impact on the substrate, and can be used for surface protection and remanufacturing of key moving parts serving in extreme marine conditions.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A copper-based amorphous powder for ultra-high-speed blue-light laser cladding, comprising the following elemental components by mass percentage:

[0010] 70-73% Cu, 10-14% Zr, 6-10% Ti, 5-9% Ni, 0.8-1.2% Si, 0.8-1.2% B.

[0011] Furthermore, the sphericity is 95-100%, the particle size distribution range is 15-75 μm, D50 is 35-55 μm, and the fluidity is 16-22 s / 50 g.

[0012] Another object of the present invention is to provide a copper-based amorphous coating for ultra-high-speed blue-light laser cladding.

[0013] A copper-based amorphous coating for ultra-high-speed blue-light laser cladding is prepared from the copper-based amorphous powder for ultra-high-speed blue-light laser cladding described in any one of the above items.

[0014] Another object of the present invention is to provide a method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding.

[0015] A method for preparing the above-mentioned copper-based amorphous coating for ultra-high-speed blue-light laser cladding comprises the following steps:

[0016] S1. depositing a copper-based amorphous powder for ultra-high-speed blue laser cladding onto the substrate surface by ultra-high-speed blue laser cladding;

[0017] S2. Grinding and polishing the surface of the substrate obtained in S1, and performing in-situ reaction heat treatment to obtain the copper-based amorphous coating for ultra-high-speed blue-light laser cladding.

[0018] Furthermore, the process parameters of the ultra-high-speed blue laser cladding described in S1 include: blue laser wavelength of 550nm, power of 1800-2200W, spot diameter of 0.8-1.2mm, powder feeding rate of 1.5-2.0kg / h, laser scanning rate of 85-100m / min, and overlap rate of 46-66%.

[0019] Furthermore, the ultra-high-speed blue light laser cladding described in S1 is performed under the protection of an inert gas.

[0020] Furthermore, the in-situ reaction heat treatment in S2 is carried out under an O2 atmosphere.

[0021] Furthermore, the process parameters of the in-situ reaction heat treatment in S2 include: heat treatment temperature of 550-900°C, O2 flow rate of 2-6sccm, and insulation time of 40-60min.

[0022] Furthermore, in the in-situ reaction heat treatment described in S2, the non-coating area is subjected to protective treatment.

[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0024] (1) The copper-based amorphous powder for ultra-high-speed blue-light laser cladding of the present invention is composed of specific elements and content ranges. Copper ions have excellent bactericidal effects and can kill marine organisms such as algae and barnacles on the surface of marine engineering equipment, making the copper-based coating have excellent anti-fouling properties; and by regulating the content of corrosion-resistant elements such as Cu, Zr, Ti, and Ni, an amorphous coating with high strength, high hardness, and high corrosion resistance can be obtained; but since laser cladding is a non-equilibrium solidification process, the formed amorphous structure is unstable and the amorphous content is limited, adding a certain amount of Si and B elements can effectively promote the stable formation of the laser cladding CuZrTiNi amorphous structure. At the same time, the laser cladding CuZrTiNi coating has many forming defects. Si and B elements have strong deoxidation and self-melting effects, which can improve the forming quality of the laser cladding CuZrTiNi coating, reduce the impurity content of the cladding layer, and significantly improve the forming quality of the cladding layer. However, if the added content of Si and B elements is less than 0.8%, the stabilization effect of the amorphous structure and the improvement effect of the forming quality are not good; if the added content of Si and B elements is too high, greater than 1.2%, they are easy to form brittle and hard inclusion phases, resulting in cracking of the coating and affecting the forming quality of the coating; therefore, the present invention has repeatedly studied and accurately adjusted the content ratio of Cu, Zr, Ti, Ni, Si, and B elements, and the obtained copper-based amorphous powder for high-speed blue light laser cladding has uniform composition, excellent sphericity and fluidity, and uniform particle size distribution. The formed amorphous structure is stable, which is very suitable for use in ultra-high-speed blue light laser cladding technology.

[0025] (2) The present invention uses powders containing specific elements and content ranges, and adopts ultra-high-speed laser cladding technology and in-situ reaction to prepare the copper-based amorphous coating for ultra-high-speed blue light laser cladding. Due to its stable amorphous structure with unique long-range disorder and short-range ordered structure, it does not have defects such as dislocations of crystalline alloys, and thus has excellent wear reduction and corrosion resistance. In addition, the release of copper ions on the surface of the coating can directly kill marine organisms such as algae and barnacles on the surface of marine engineering equipment, and has excellent anti-fouling performance.

[0026] (3) The copper-based amorphous coating for ultra-high-speed blue-light laser cladding of the present invention is prepared by blue-light ultra-high-speed laser cladding technology. Since copper alloy has high reflectivity and low energy absorption for traditional long-wavelength red-light laser cladding, defects are easily formed in the coating. The present invention innovatively adopts short-wavelength blue-light laser cladding, which greatly improves the absorption rate of copper alloy to laser energy, which is more than 10 times higher than the red-light laser absorption rate, thereby significantly improving the forming quality of the copper-based amorphous coating for ultra-high-speed blue-light laser cladding. The preparation method is efficient, easy to operate, low in cost, has little thermal impact on the substrate, forms a metallurgical bond with the substrate, and the prepared copper-based amorphous coating for ultra-high-speed blue-light laser cladding is dense and defect-free. The obtained coating can be used for surface protection and remanufacturing of key moving parts serving in extreme marine conditions, has important economic value and promotion significance, and has good application prospects in the fields of marine engineering equipment, rail transit, metallurgy, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] The invention is further described using the accompanying drawings, but the embodiments in the accompanying drawings do not constitute any limitation to the invention. A person skilled in the art can obtain other drawings based on the following drawings without creative work.

[0028] Figure 1 This is an electron microscope image of the copper-based amorphous powder used for ultra-high-speed blue light laser cladding in Example 1 of the present application.

[0029] Figure 2 This is the XRD test result of the copper-based amorphous coating for ultra-high-speed blue light laser cladding in Example 1 of the present application. DETAILED DESCRIPTION

[0030] In order to better illustrate the purpose, technical scheme and advantages of the present invention, the present invention is further described by the following examples. Obviously, the following examples are only part of the embodiments of the present invention, rather than all the embodiments; it should be understood that the embodiments of the present invention are only used to illustrate the technical effects of the present invention, rather than to limit the scope of protection of the present invention.

[0031] The raw materials in the examples can all be obtained commercially; unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0032] Example 1

[0033] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding comprises the following steps:

[0034] S1. 70% Cu, 10% Zr, 9% Ti, 9% Ni, 1% Si, 1% B copper-based amorphous powder for ultra-high-speed blue-light laser cladding is deposited on the surface of the substrate by ultra-high-speed blue-light laser cladding, wherein the copper-based amorphous powder for ultra-high-speed blue-light laser cladding has a sphericity of 95%, a particle size distribution range of 15-75 μm, a D50 of 45 μm, and a fluidity of 18 s / 50 g. The process parameters of the ultra-high-speed blue-light laser cladding include: a blue laser wavelength of 550 nm, a power of 2000 W, a spot diameter of 1 mm, a powder feeding rate of 1.8 kg / h, a laser scanning rate of 90 m / min, an overlap rate of 50%, and inert gas protection during the ultra-high-speed laser cladding process;

[0035] S2. The substrate surface obtained in S1 is ground and polished, and then placed in a heat treatment furnace. O2 is then introduced into the heat treatment furnace for in-situ reaction heat treatment. The heat treatment temperature is 550-900°C, the flow rate of O2 is 3sccm, and the holding time is 50min. The non-coating area is protected to obtain the copper-based amorphous coating for ultra-high-speed blue light laser cladding.

[0036] Example 2

[0037] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0038] Compared with Example 1, the copper-based amorphous powder for ultra-high-speed blue laser cladding contains 73% Cu, 10% Zr, 6.3% Ti, 8.3% Ni, 1.2% Si and 1.2% B.

[0039] Example 3

[0040] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0041] Compared with Example 1, the laser power of S1 ultra-high-speed blue-light laser cladding is 2200W.

[0042] Example 4

[0043] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0044] Compared with Example 1, the scanning speed of S1 ultra-high-speed blue light laser cladding is 100 m / min.

[0045] Comparative Example 1

[0046] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0047] Compared with Example 1, the copper-based amorphous powder for ultra-high-speed blue laser cladding in this comparative example contains 70% Cu, 10% Zr, 9% Ti, 9% Ni, 0% Si and 1% B, that is, does not contain Si element.

[0048] Comparative Example 2

[0049] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0050] Compared with Example 1, the copper-based amorphous powder for ultra-high-speed blue laser cladding in this comparative example contains 70% Cu, 10% Zr, 9% Ti, 9% Ni, 1% Si and 0% B, that is, does not contain the B element.

[0051] Comparative Example 3

[0052] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0053] Compared with Example 1, the copper-based amorphous powder for ultra-high-speed blue laser cladding in this comparative example contains 70% Cu, 10% Zr, 8% Ti, 9% Ni, 2% Si and 1% B, that is, the Si element is excessive.

[0054] Comparative Example 4

[0055] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0056] Compared with Example 1, the copper-based amorphous powder for ultra-high-speed blue laser cladding in this comparative example contains 70% Cu, 10% Zr, 8% Ti, 9% Ni, 1% Si and 2% B, that is, the B element is excessive.

[0057] Comparative Example 5

[0058] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0059] Compared with Example 1, the sphericity of the copper-based amorphous powder for ultra-high-speed blue-light laser cladding in this comparative example is 60%.

[0060] Comparative Example 6

[0061] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0062] Compared with Example 1, the D50 of the copper-based amorphous powder for ultra-high-speed blue-light laser cladding in this comparative example is 5 μm.

[0063] Comparative Example 7

[0064] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0065] Compared with Example 1, the D50 of the copper-based amorphous powder for ultra-high-speed blue-light laser cladding in this comparative example is 100 μm.

[0066] Comparative Example 8

[0067] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0068] Compared with Example 1, in step S1 of this comparative example, ultra-high-speed red-light laser cladding is used to deposit copper-based amorphous powder for ultra-high-speed blue-light laser cladding on the surface of the substrate.

[0069] Comparative Example 9

[0070] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0071] Compared with Example 1, step S2 of this comparative example does not perform in-situ reaction heat treatment.

[0072] Comparative Example 10

[0073] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0074] Compared with Example 1, the ultra-high-speed blue-light laser cladding process parameters in step S1 of this comparative example are: laser power 1000W.

[0075] Comparative Example 11

[0076] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0077] Compared with Example 1, the ultra-high-speed blue-light laser cladding process parameters in step S1 of this comparative example are: laser power 4000W.

[0078] Comparative Example 12

[0079] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0080] Compared with Example 1, the ultra-high-speed blue-light laser cladding process parameters in step S1 of this comparative example are: scanning speed 60 m / min.

[0081] Comparative Example 13

[0082] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0083] Compared with Example 1, the ultra-high-speed blue-light laser cladding process parameters in step S1 of this comparative example are: scanning speed 120 m / min.

[0084] Comparative Example 14

[0085] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0086] Compared with Example 1, in the ultra-high-speed blue-light laser cladding process in step S1 of this comparative example, inert atmosphere protection is not performed.

[0087] Comparative Example 15

[0088] A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, wherein the steps not specifically described are the same as those in Example 1, except that:

[0089] Compared with Example 1, the in-situ reaction heat treatment temperature in step S2 of this comparative example is 300°C.

[0090] Figure 2 This is the XRD test result of the copper-based amorphous coating for ultra-high-speed blue-light laser cladding in Example 1 of the present application. It can be observed that the coating forms a stable long-range disordered and short-range ordered amorphous structure.

[0091] The characterization test results of the remaining embodiments are basically consistent with those of Embodiment 1.

[0092] The above samples were subjected to performance tests, and the experimental test methods were as follows:

[0093] Test method for coating forming quality: Determined in accordance with the national standard "GB / T 36591-2018"

[0094] Test method for wear weight loss: Determined in accordance with the national standard "GB / T 12444-2006"

[0095] Corrosion rate test method: Determined in accordance with the national standard "GB / T 40299-2021"

[0096] Microhardness test method: Determined in accordance with the national standard "GB / T 4342-1991"

[0097] Anti-biological fouling test method: refer to the national standard "GB / T5370-2007" test

[0098] Among them, the microhardness indicates the hardness of the coating, and the larger the value, the higher the hardness of the coating; the wear loss weight indicates the wear resistance of the coating, and the smaller the value, the better the wear resistance of the coating; the corrosion rate indicates the corrosion resistance of the coating, and the smaller the value, the better the corrosion resistance of the coating; the fouling wet weight indicates the anti-fouling performance of the coating, and the smaller the value, the better the anti-fouling performance of the coating.

[0099] The test results of Examples 1-4 and Comparative Examples 1-15 are shown in the following table:

[0100] Table 1 Test results of Examples 1-4 and Comparative Examples 1-15

[0101]

[0102]

[0103] It can be seen from Table 1 that the coatings in the embodiments of the present invention have good forming quality and no defects, the weight loss from abrasion is less than 35 mg, and the corrosion rate can be as low as 0.06 mm·a. -1 , the wet weight of the pollution is 600g·m -2 It has outstanding comprehensive performance compared with the comparative examples, indicating that the copper-based amorphous coating for ultra-high-speed blue light laser cladding of the present invention has excellent corrosion resistance, abrasion resistance and anti-fouling properties.

[0104] However, due to the lack of Si and B elements, the forming quality of Comparative Examples 1 and 2 is poor, the microhardness is greatly reduced, and the wear loss is higher than 80 mg; due to the excessive Si and B elements, the forming quality of Comparative Examples 3 and 4 is poor, and the corrosion rate is high; Comparative Examples 5, 6, and 7 change the powder sphericity and D50, resulting in poor coating forming quality, many defects, and a high corrosion rate; Comparative Example 8 uses an ultra-high-speed red light laser cladding method, and the resulting coating quality is the worst among all the embodiments and comparative examples, with low microhardness, high wear loss, and a corrosion rate as high as 1.21 mm·a -1 , the wet weight of the fouling is up to 1355g·m -2 Comparative Example 9 did not undergo in-situ reaction heat treatment, and the wet weight of the contamination was 1234 g·m -2, the antifouling performance is poor; comparative examples 10, 11, 12, and 13 change the ultra-high-speed blue-light laser cladding process parameters, and the corrosion resistance and abrasion resistance are not good; comparative example 14 does not perform inert atmosphere protection, and the comprehensive performance is acceptable among the comparative examples, but it is far from being comparable to the embodiments; comparative example 15 in-situ reaction heat treatment temperature exceeds the range, and the antifouling performance is poor. It shows that the ultra-high-speed blue-light laser cladding copper-based amorphous coating obtained by ultra-high-speed blue-light laser cladding through specific ultra-high-speed blue-light laser cladding of the present invention, which is composed of ultra-high-speed blue-light laser cladding copper-based amorphous powder composed of specific elements and content ranges, has significantly excellent comprehensive performance.

[0105] In summary, the copper-based amorphous powder for ultra-high-speed blue-light laser cladding of the present invention is composed of specific elements and content ranges, and the content ratio of Cu, Zr, Ti, Ni, Si, and B elements is precisely controlled. The obtained copper-based amorphous powder for ultra-high-speed blue-light laser cladding has uniform composition, excellent sphericity and fluidity, and uniform particle size distribution. The formed amorphous structure is stable, has excellent sterilization effect, high strength, high hardness, high corrosion resistance, and high coating forming quality; the ultra-high-speed blue-light laser cladding copper-based amorphous coating for ultra-high-speed blue-light laser cladding prepared by the powder using ultra-high-speed laser cladding technology and in-situ reaction has a stable amorphous structure with unique long-range The disordered, short-range ordered structure does not have defects such as dislocations in crystalline alloys, and thus has excellent wear reduction and corrosion resistance. The specific short-wavelength blue light laser cladding is used to greatly improve the absorption rate of laser energy by copper alloy, which is more than 10 times higher than the red light laser absorption rate, thereby significantly improving the forming quality of the copper-based amorphous coating for ultra-high-speed blue light laser cladding. The preparation method is efficient, easy to operate, low in cost, has little thermal impact on the substrate, forms a metallurgical bond with the substrate, and the copper-based amorphous coating for ultra-high-speed blue light laser cladding is dense and defect-free, which has important economic value and promotion significance, and has good application prospects in marine engineering equipment, rail transit, metallurgy and other fields.

[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention, rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding, characterized in that: The following steps are involved: S1. depositing a copper-based amorphous powder for ultra-high-speed blue laser cladding onto the substrate surface by ultra-high-speed blue laser cladding; S2. The surface of the substrate obtained in S1 is ground and polished, and subjected to in-situ reaction heat treatment to obtain the copper-based amorphous coating for ultra-high-speed blue-light laser cladding; The copper-based amorphous powder for ultra-high-speed blue-light laser cladding comprises the following elemental components by mass percentage: 70-73% Cu, 10-14% Zr, 6-10% Ti, 5-9% Ni, 0.8-1.2% Si, 0.8-1.2% B; The copper-based amorphous powder for ultra-high-speed blue-light laser cladding has a sphericity of 95-100%, a particle size distribution range of 15-75 μm, a D50 of 35-55 μm, and a fluidity of 16-22 s / 50 g; The process parameters of the ultra-high-speed blue laser cladding described in S1 include: blue laser wavelength of 550nm, power of 1800-2200W, spot diameter of 0.8-1.2mm, powder feeding rate of 1.5-2.0kg / h, laser scanning rate of 85-100m / min, and overlap rate of 46-66%; The ultra-high-speed blue-light laser cladding described in S1 is carried out under the protection of an inert gas; The process parameters of the in-situ reaction heat treatment described in S2 include: heat treatment temperature of 550-900°C, O2 flow rate of 2-6sccm, and insulation time of 40-60min.

2. A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding according to claim 1, characterized in that: The in-situ reaction heat treatment described in S2 is carried out under an O2 atmosphere.

3. A method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding according to claim 1, characterized in that: In the in-situ reaction heat treatment described in S2, the non-coating area is subjected to protective treatment.

4. A copper-based amorphous coating for ultra-high-speed blue-light laser cladding, characterized in that: The coating is prepared by the method for preparing a copper-based amorphous coating for ultra-high-speed blue-light laser cladding as described in any one of the above items.