Polymer battery copper current collector and preparation method thereof
By using materials such as zinc nitrate, aluminum nitrate and acrylamide, AZO targets are prepared, and the copper foil surface is modified through sputtering coating technology, the copper foil surface modification cost and poor interface stability in the prior art are solved. The problem is that uniform deposition of lithium ions and stable improvement of battery interfaces has been achieved.
Patent Information
- Application Number
- CN202311778686.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2043-12-22
AI Technical Summary
The prior art has problems such as high cost, difficult process and poor interface stability in improving the surface modification of copper foil current collector of lithium-ion batteries, which affects the uniformity of lithium-ion deposition and the safety of battery operation.
Zinc nitrate, aluminum nitrate, acrylamide and N-N'methylenebisacrylamide are used to form a solution, and the gel is formed after reaction of the initiator. After drying, it is calcined to obtain the AZO precursor, and the AZO target is prepared by ball milling and sintering. The imaging coating technology modifies the surface of the copper foil to form a thin and uniform AZO modification layer.
Reduces the lithium ion nucleation barrier, improves the uniform distribution of lithium ions on the surface of the foil, reduces the difficulty and cost of preparation, enhances the interface stability and lithium-philicity of copper foil, avoids the growth of lithium dendrites, and ensures that The uniformity of the surface morphology and composition of the foil material.
Smart Images

Figure BDA0004623078330000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of surface modification of copper foil current collectors, and in particular relates to a polymer battery copper current collector and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have flourished over the past three decades due to their high energy density, no memory effect, and safety. With the large-scale application of new energy vehicles, mobile digital products, and smart phones, traditional lithium-ion batteries are gradually unable to meet the needs of the rapidly developing energy market. The main reason why traditional lithium-ion batteries cannot break through the energy density bottleneck is that the energy density of the graphite negative electrode is low. Among the many negative electrode materials, lithium metal is considered to be the best choice for negative electrode materials due to its extremely high theoretical specific capacity and lowest potential (-3.04V compared to the standard hydrogen electrode).
[0003] Using ultra-thin lithium foil as the negative electrode can greatly increase the energy density. In addition to the strict requirements on the processing environment, the technical difficulty lies in how to improve the uniformity of lithium ion deposition on the negative electrode current collector during charging to ensure the interface stability during battery operation. Copper foil is the most widely used negative electrode current collector material for lithium batteries. Its advantages are good electrochemical stability and good conductivity, but the "lithium repellency" of metallic copper makes the overpotential of lithium ions on the surface of copper foil high, resulting in low deposition efficiency and easily causing uneven distribution of lithium ions on the surface of the foil, which affects nucleation and causes the growth of lithium dendrites, causing interface failure and affecting battery operation safety.
[0004] In recent years, introducing a modified layer on the surface of copper foil is an effective method to improve the interface stability. The most common modification method is to modify the surface of copper foil with a layer of lithium-philic metal to reduce the nucleation overpotential of lithium and promote the stable deposition and stripping of lithium ions. However, the high cost has limited the development of such solutions. At the same time, surface carbon layer and polymer layer modification are also commonly used to modify the surface of copper foil, but its high process difficulty is not conducive to mass production. In addition, porous structured current collectors are also used to stabilize the negative electrode interface. The disadvantage is that the surface area is too large, which will affect the stability of the negative electrode SEI film.
[0005] It can be seen that using a simple process and low-cost method to modify the surface of copper foil current collector is of great significance for improving the energy density of lithium-ion batteries. Scholars and personnel in related fields are also constantly researching. For example, the Chinese invention patent with announcement number CN111969212A proposes to introduce a lithium-philic metal layer to modify the surface of copper foil, which can induce uniform deposition of lithium and reduce the risk of lithium dendrites. The invention patent with announcement number CN108767263A discloses a method for in-situ growth of Zn-MOF two-dimensional nanosheet arrays on copper foil current collectors for modification. This coating layer effectively increases the interface contact area and improves deposition efficiency. However, these existing methods have the following disadvantages: (1) The cost of using metal as the lithium-philic layer is relatively high, and the disadvantage of modification by magnetron sputtering is that the utilization rate of the metal target is not high and the target preparation is difficult, which further increases the cost and is not suitable for large-scale application on copper foil; (2) The in-situ growth of the MOF layer has strict requirements on the growth environment and is not easy to achieve in large-scale production. In addition, the thickness of the in-situ modified layer is difficult to control, and surface shedding cannot be avoided during the winding process of the pole piece, resulting in poor process stability; (3) The surface area of the in-situ grown modified layer is closely related to the interface stability. The disadvantages of its uncontrollable surface area and surface morphology will amplify the problems between the interface and the electrolyte, resulting in uneven growth of the SEI film and causing interface degradation. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a surface modification method of a copper foil current collector which can ensure the uniformity of the foil surface morphology and composition and improve the lithium affinity of the foil, and a copper current collector prepared by using the modification method.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a copper current collector for a polymer battery, comprising the following steps:
[0008] S1, preparing a solution of zinc nitrate, aluminum nitrate, acrylamide and N-N'methylenebisacrylamide, adding an initiator to react to obtain a gel, and drying the gel to obtain an AZO precursor;
[0009] S2, calcining the AZO precursor to obtain AZO powder; mixing the AZO powder with anhydrous ethanol and then ball milling, then evaporating the ethanol to prepare a target material embryo, and then sintering to obtain an AZO target;
[0010] S3. Use AZO target material to sputter-coat the surface of copper foil to obtain copper current collector for polymer battery.
[0011] Another technical solution adopted by the present invention is: a polymer battery copper current collector prepared by the above-mentioned preparation method of the polymer battery copper current collector.
[0012] The beneficial effects of the present invention are as follows: the preparation method provided by the present invention uses acrylamide and N-N'methylenebisacrylamide in combination with a specific process to prepare an AZO target material, which is used to perform surface modification on a copper foil, and the formed AZO modified layer has a small thickness, and can promote the uniform distribution of lithium ions on the foil surface without affecting the interface impedance. Compared with a pure metal target layer, the preparation difficulty is smaller, the raw material reserves are abundant, the cost is lower, and AZO is non-toxic, has good high-temperature stability, excellent conductivity, and good adhesion to the copper foil. DETAILED DESCRIPTION
[0013] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in conjunction with the implementation modes.
[0014] The method for preparing a copper current collector for a polymer battery comprises the following steps:
[0015] S1, preparing a solution of zinc nitrate, aluminum nitrate, acrylamide and N-N'methylenebisacrylamide, adding an initiator to react to obtain a gel, and drying the gel to obtain an AZO precursor;
[0016] S2, calcining the AZO precursor to obtain AZO powder; mixing the AZO powder with anhydrous ethanol and then ball milling, then evaporating the ethanol to prepare a target material embryo, and then sintering to obtain an AZO target;
[0017] S3. Use AZO target material to sputter-coat the surface of copper foil to obtain copper current collector for polymer battery.
[0018] From the above description, it can be seen that the beneficial effect of the present invention is that: the present invention adopts acrylamide and N-N'methylenebisacrylamide as polymers and cooperates with a specific process to make an AZO target material, and the obtained AZO target material has high purity, high density and good uniformity, and then during the subsequent sputtering coating, it can ensure good adhesion between the modified layer and the copper foil, and form a thin and uniform modified layer.
[0019] Further, the molar ratio of zinc to aluminum is 1:100 to 10:100. Preferably, the molar ratio of zinc to aluminum is 1 to 2:100.
[0020] Furthermore, the mass ratio of acrylamide to N-N'methylenebisacrylamide is 15:1 to 20:1.
[0021] From the above description, it can be seen that acrylamide and N-N'methylenebisacryl do not react with the components in the mixed solution. After acrylamide and N-N'methylenebisacryl are added, the N-N'methylenebisacryl chain segments carry cross-linking groups, which react with the acrylamide polymer. The effect brought about is that the linear monomer acrylamide forms a three-dimensional network gel structure after cross-linking. The formation of the three-dimensional network gel structure quickly fixes the components in the solution in space, and can achieve uniform mixing of various component elements at the atomic level in the aqueous solution, improve the chemical uniformity of the powder, reduce the molecular aggregation effect, and reduce agglomeration. The present invention selects acrylamide as a monomer and N-N'methylenebisacryl as a cross-linking agent. The components in the mixed solution are quickly fixed in the spatial three-dimensional structure composed of the two, reducing the probability of intermolecular contact and reducing agglomeration. Compared with other cross-linking agents, the AZO target material finally prepared has better uniformity.
[0022] Furthermore, the S1 is specifically:
[0023] S1.1, respectively preparing a zinc nitrate aqueous solution and an aluminum nitrate aqueous solution using zinc nitrate and aluminum nitrate, and mixing the two to obtain a zinc-aluminum nitrate mixed solution;
[0024] S1.2, adding acrylamide and N-N'-methylenebisacrylamide to the zinc nitrate aluminum mixed solution, stirring until the solution is clear, then adding an initiator, and completing the cross-linking reaction under heating conditions to obtain a gel;
[0025] S1.3. Dry the gel to obtain AZO precursor.
[0026] Further, the initiator is preferably 0.5 wt % of ammonium persulfate.
[0027] From the above description, it can be seen that the initiator ammonium persulfate will generate primary free radicals in a high-temperature water bath. The free radicals attack the double bonds in the acrylamide structure, causing free radical polymerization between acrylamide molecules to form long-chain molecules. The long-chain molecules then undergo cross-linking reaction with N-N'methylenebisacrylamide to form a gel.
[0028] Furthermore, the total mass of acrylamide and N-N'methylenebisacrylamide in S1.2 is 3-8% of the total mass of the zinc-aluminum nitrate mixed solution.
[0029] Furthermore, the heating condition in S1.2 is water bath heating, the water bath temperature is 75-80° C., and the time is 20-40 min. The stirring in S1.2 is carried out at room temperature, the stirring speed is 200-500 r / min, preferably 300 r / min, and the stirring can be magnetic stirring.
[0030] From the above description, it can be seen that the cross-linking reaction can only be completed under high temperature, and the cross-linking reaction can be completed in 20 to 40 minutes at the above temperature.
[0031] Furthermore, in S1.3, the gel is placed in a vacuum drying oven at 85 to 90° C. for 48 to 72 hours.
[0032] From the above description, it can be seen that drying is used to remove water from the gel to obtain an AZO precursor. The water removal efficiency is high within this temperature and time range, and it can avoid the problem of gel network pyrolysis caused by excessive temperature, destruction of the three-dimensional structure, and particle agglomeration.
[0033] Furthermore, the calcination in S2 is specifically as follows: vacuum calcination is performed from room temperature to 350-500°C (preferably 450°C) at 0.5-0.6 kPa, and then kept warm for 3-3.5h (preferably 3h) in an inert gas environment, with a heating rate of 8-12°C / min (preferably 10°C / min).
[0034] From the above description, it can be seen that by calcining at the above pressure and temperature, the side chains and main chains of acrylamide and N-N'methylenebisacryl are thermally decomposed and removed. The control of temperature and heating rate during calcination also plays a key role. When the heating rate is slower at 8-12°C / min, the grains can grow more orderly and the pores can be slowly eliminated, but the rate should not be slower, which will cause too much time and increase the cost; when the heating rate exceeds 12°C / min, the internal crystal phase cannot grow densely, and the internal pores cannot be discharged in time, resulting in a significant decrease in density. The selection of the above temperature range can well balance the cost and target density. By adjusting the calcination process, high-purity, high-density AZO powder is obtained, and then a target with uniform particle size distribution and good uniformity is prepared.
[0035] Furthermore, in S2, AZO powder and anhydrous ethanol are mixed in a volume ratio of 1:1 and then ball-milled, using zirconium oxide balls as ball milling beads, the volume ratio of ball milling beads to materials (AZO powder and anhydrous ethanol) is 1.2:1, the ball milling time is 24 hours, and after ball milling, it is placed in an oven at 60° C. to dry and remove ethanol.
[0036] From the above description, it can be seen that ball milling can further reduce the particle size of AZO powder and improve the uniformity of sintering. The drying temperature after ball milling should not be too high, and drying at a higher temperature will cause the powder to agglomerate.
[0037] Furthermore, the sintering in S2 is specifically as follows: placing the target material embryo into a vacuum hot pressing sintering furnace, turning on the vacuum pump to evacuate until the vacuum degree reaches 10 -1 Up to 10 -2Pa, pressurized to 120MPa, sintering temperature of 1250℃~1300℃, heating rate of 8~12℃ / min (preferably 10℃ / min), sintering time of 3~4h, and naturally cooled to room temperature after sintering to obtain AZO target.
[0038] From the above description, it can be seen that, like the calcining process, reasonable control of the temperature and heating rate during the sintering process can ensure the high density of the target material, so as to obtain a target material with uniform particle size distribution and good uniformity.
[0039] Further, S3 is specifically as follows: pasting the copper foil on the glass substrate, controlling the distance between the AZO target and the glass substrate to be 50-60 mm, raising the temperature of the glass substrate to 200°C; and then evacuating the glass substrate to a vacuum degree of 5×10 -4 Pa, sputtering was performed using a radio frequency power supply with a power of 150 to 200 W and a sputtering time of 30 min.
[0040] From the above description, it can be seen that the magnetron sputtering coating method has strong stability and uniformity, simple process, suitable for factory batch production, and can ensure the uniformity of the foil surface morphology and composition to the greatest extent.
[0041] Furthermore, after the sputtering coating, an annealing step is also included. The annealing is specifically as follows: the glass substrate is heated to 300° C. and kept for 3 minutes, and then the substrate is removed after the temperature naturally drops to room temperature.
[0042] From the above description, it can be seen that after AZO is sputtered on the copper foil, it exists in an amorphous state, has poor crystallinity, and has many internal defects. The present invention can improve the crystallinity of the AZO film on the copper foil and reduce internal defects by adopting a higher annealing step of 300°C for 3h.
[0043] Another technical solution of the present invention is: a polymer battery copper current collector prepared according to any of the above-mentioned preparation methods of polymer battery copper current collectors.
[0044] From the above description, it can be seen that the beneficial effects of the present invention are: the AZO prepared by the present invention can form a Li-Zn alloy with lithium on the surface, thereby improving the lithium affinity of the foil, and further reducing the nucleation barrier of lithium ions during the charge and discharge process; at the same time, it can greatly reduce the work function of the electrode surface, improve the reduction ability of lithium ions in the electrolyte at the interface, avoid uneven local charge distribution, thereby promoting the uniform deposition of lithium on the copper foil surface, and accelerate the process of forming a stable SEI film on the interface at the early stage of the cycle, while ensuring the uniformity of the surface morphology and composition of the foil.
[0045] Embodiment 1 of the present invention is: a method for preparing a copper current collector for a polymer battery, comprising the following steps:
[0046] S1.1, respectively preparing a zinc nitrate aqueous solution and an aluminum nitrate aqueous solution with zinc nitrate and aluminum nitrate, and mixing the two to obtain a zinc-aluminum nitrate mixed solution; the molar ratio of zinc to aluminum in the zinc-aluminum nitrate mixed solution is 1.5:100;
[0047] S1.2, add 8% of the total mass of acrylamide and N-N'methylenebisacrylamide to the zinc nitrate aluminum mixed solution, the mass ratio of acrylamide to N-N'methylenebisacrylamide is 20:1, stir magnetically at 300 r / min for 10 min until the solution is clear, then add 0.5wt% of ammonium persulfate, and complete the cross-linking reaction in a water bath at 80°C to obtain a gel;
[0048] S1.3, placing the gel in a vacuum drying oven and drying at 90°C for 52 h to obtain an AZO precursor;
[0049] S2.1. Place the AZO precursor in a corundum boat, increase the vacuum sintering pressure from room pressure to 0.5 kPa, then increase the temperature from room temperature to 450 °C for vacuum calcination, and then keep the temperature in an inert gas environment for 3 h at a heating rate of 10 °C / min to obtain AZO powder;
[0050] S2.2, AZO powder and anhydrous ethanol were mixed in a volume ratio of 1:1 and then ball-milled, with zirconium oxide balls as ball milling beads, the volume ratio of ball milling beads to materials (AZO powder and anhydrous ethanol) was 1.2:1, the ball milling time was 24h, and after ball milling, the mixture was placed in an oven at 60°C to dry and remove ethanol, thereby obtaining a target embryo;
[0051] S2.3. Place the target material embryo into a vacuum hot pressing sintering furnace and turn on the vacuum pump to evacuate until the vacuum degree reaches 10 - 1 Pa, pressurized to 120MPa, sintered at 1250℃, heated at 10℃ / min, sintered for 3.5h, and cooled to room temperature naturally after sintering to obtain AZO target;
[0052] S3.1. Paste the copper foil on the glass substrate. The distance between the AZO target and the glass substrate is controlled at 50-60 mm. Raise the temperature of the glass substrate to 200 °C. Then evacuate the glass substrate to a vacuum degree of 5 × 10 -4 Pa, sputtering was performed using a radio frequency power supply with a power of 200 W and a sputtering time of 30 min;
[0053] S3.2. After the sputtering is completed, the temperature of the glass substrate is raised to 300°C and kept at this temperature for 3 minutes, then the glass substrate is removed to obtain the copper current collector of the polymer battery.
[0054] Embodiment 2 of the present invention is: a method for preparing a copper current collector for a polymer battery, comprising the following steps:
[0055] S1.1, respectively preparing a zinc nitrate aqueous solution and an aluminum nitrate aqueous solution with zinc nitrate and aluminum nitrate, and mixing the two to obtain a zinc-aluminum nitrate mixed solution; the molar ratio of zinc to aluminum in the zinc-aluminum nitrate mixed solution is 2100;
[0056] S1.2, add 3% of the total mass of acrylamide and N-N'methylenebisacrylamide to the zinc nitrate aluminum mixed solution, the mass ratio of acrylamide to N-N'methylenebisacrylamide is 18:1, stir magnetically at 500 r / min for 10 min until the solution is clear, then add 0.5wt% of ammonium persulfate, and complete the cross-linking reaction in a water bath at 80°C to obtain a gel;
[0057] S1.3, placing the gel in a vacuum drying oven and drying at 90°C for 48 h to obtain an AZO precursor;
[0058] S2.1. Place the AZO precursor in a corundum boat, increase the vacuum sintering pressure from the room pressure to 0.6 kPa, then increase the temperature from room temperature to 400 °C for vacuum calcination, and then keep the temperature in an inert gas environment for 3.2 h at a heating rate of 12 °C / min to obtain AZO powder;
[0059] S2.2, AZO powder and anhydrous ethanol were mixed in a volume ratio of 1:1 and then ball-milled, with zirconium oxide balls as ball milling beads, the volume ratio of ball milling beads to materials (AZO powder and anhydrous ethanol) was 1.2:1, the ball milling time was 24h, and after ball milling, the mixture was placed in an oven at 60°C to dry and remove ethanol, thereby obtaining a target embryo;
[0060] S2.3. Place the target material embryo into a vacuum hot pressing sintering furnace and turn on the vacuum pump to evacuate until the vacuum degree reaches 10 - 1 Pa, pressurized to 120MPa, sintered at 1300℃, heated at 12℃ / min, sintered for 3.2h, and cooled to room temperature naturally after sintering to obtain AZO target;
[0061] S3.1. Paste the copper foil on the glass substrate. The distance between the AZO target and the glass substrate is controlled at 50-60 mm. Raise the temperature of the glass substrate to 200 °C. Then evacuate the glass substrate to a vacuum degree of 5 × 10 -4 Pa, sputtering was performed using a radio frequency power supply with a power of 150 W and a sputtering time of 30 min;
[0062] S3.2. After the sputtering is completed, the temperature of the glass substrate is raised to 300°C and kept at this temperature for 3 minutes, then the glass substrate is removed to obtain the copper current collector of the polymer battery.
[0063] Embodiment 3 of the present invention is: a method for preparing a copper current collector for a polymer battery, comprising the following steps:
[0064] S1.1, respectively preparing a zinc nitrate aqueous solution and an aluminum nitrate aqueous solution with zinc nitrate and aluminum nitrate, and mixing the two to obtain a zinc-aluminum nitrate mixed solution; the molar ratio of zinc to aluminum in the zinc-aluminum nitrate mixed solution is 1:100;
[0065] S1.2, add 5% of the total mass of acrylamide and N-N'methylenebisacrylamide to the zinc nitrate aluminum mixed solution, the mass ratio of acrylamide to N-N'methylenebisacrylamide is 15:1, stir magnetically at 200 r / min for 10 min until the solution is clear, then add 0.5wt% of ammonium persulfate, and heat in a water bath at 75°C to complete the cross-linking reaction to obtain a gel;
[0066] S1.3, placing the gel in a vacuum drying oven and drying at 85°C for 72 h to obtain an AZO precursor;
[0067] S2.1. Place the AZO precursor in a corundum boat, increase the pressure of the vacuum sintering furnace from room temperature to 0.55 kPa, then increase the temperature from room temperature to 500 °C for vacuum calcination, and then keep the temperature in an inert gas environment for 3 h at a rate of 8 °C / min to obtain AZO powder;
[0068] S2.2, AZO powder and anhydrous ethanol were mixed in a volume ratio of 1:1 and then ball-milled, with zirconium oxide balls as ball milling beads, the volume ratio of ball milling beads to materials (AZO powder and anhydrous ethanol) was 1.2:1, the ball milling time was 24h, and after ball milling, the mixture was placed in an oven at 60°C to dry and remove ethanol, thereby obtaining a target embryo;
[0069] S2.3. Place the target material embryo into a vacuum hot pressing sintering furnace and turn on the vacuum pump to evacuate until the vacuum degree reaches 10 - 1 Pa, pressurized to 120MPa, sintered at 1280℃, heated at 8℃ / min, sintered for 4h, and cooled to room temperature naturally after sintering to obtain AZO target;
[0070] S3.1. Paste the copper foil on the glass substrate. The distance between the AZO target and the glass substrate is controlled at 50-60 mm. Raise the temperature of the glass substrate to 200 °C. Then evacuate the glass substrate to a vacuum degree of 5 × 10 -4 Pa, sputtering was performed using a radio frequency power supply with a power of 180 W and a sputtering time of 30 min;
[0071] S3.2. After the sputtering is completed, the temperature of the glass substrate is raised to 300°C and kept at this temperature for 3 minutes, then the glass substrate is removed to obtain the copper current collector of the polymer battery.
[0072] Embodiment 4 of the present invention is: a method for preparing a copper current collector for a polymer battery, comprising the following steps:
[0073] S1.1, respectively preparing a zinc nitrate aqueous solution and an aluminum nitrate aqueous solution with zinc nitrate and aluminum nitrate, and mixing the two to obtain a zinc-aluminum nitrate mixed solution; the molar ratio of zinc to aluminum in the zinc-aluminum nitrate mixed solution is 10:100;
[0074] S1.2, add 7% of the total mass of acrylamide and N-N'methylenebisacrylamide to the zinc nitrate aluminum mixed solution, the mass ratio of acrylamide to N-N'methylenebisacrylamide is 17:1, stir magnetically at 400 r / min for 10 min until the solution is clear, then add 0.5wt% of ammonium persulfate, and heat in a water bath at 80°C to complete the cross-linking reaction to obtain a gel;
[0075] S1.3, placing the gel in a vacuum drying oven and drying at 90°C for 52 h to obtain an AZO precursor;
[0076] S2.1. Place the AZO precursor in a corundum boat, increase the vacuum sintering pressure from room pressure to 0.6 kPa, then increase the temperature from room temperature to 350 °C for vacuum calcination, and then keep the temperature in an inert gas environment for 3.5 h at a heating rate of 10 °C / min to obtain AZO powder;
[0077] S2.2, AZO powder and anhydrous ethanol were mixed in a volume ratio of 1:1 and then ball-milled, with zirconium oxide balls as ball milling beads, the volume ratio of ball milling beads to materials (AZO powder and anhydrous ethanol) was 1.2:1, the ball milling time was 24h, and after ball milling, the mixture was placed in an oven at 60°C to dry and remove ethanol, thereby obtaining a target embryo;
[0078] S2.3. Place the target material embryo into a vacuum hot pressing sintering furnace and turn on the vacuum pump to evacuate until the vacuum degree reaches 10 - 1 Pa, pressurized to 120MPa, sintered at 1250℃, heated at 10℃ / min, sintered for 3.5h, and cooled to room temperature naturally after sintering to obtain AZO target;
[0079] S3.1. Paste the copper foil on the glass substrate. The distance between the AZO target and the glass substrate is controlled at 50-60 mm. Raise the temperature of the glass substrate to 200 °C. Then evacuate the glass substrate to a vacuum degree of 5 × 10 -4 Pa, sputtering was performed using a radio frequency power supply with a power of 200 W and a sputtering time of 30 min;
[0080] S3.2. After the sputtering is completed, the temperature of the glass substrate is raised to 300°C and kept at this temperature for 3 minutes, then the glass substrate is removed to obtain the copper current collector of the polymer battery.
[0081] Comparative Example 1 is as follows: The only difference between Comparative Example 1 and Example 1 is that the monomer divinylbenzene and the cross-linking agent ethylene glycol dimethacrylate are used instead of acrylamide and N-N'methylenebisacrylamide.
[0082] Comparative Example 2 is as follows: The only difference between Comparative Example 2 and Example 1 is that the AZO precursor is not calcined but is directly mixed with anhydrous ethanol and ball-milled.
[0083] Comparative Example 3 is as follows: The only difference between Comparative Example 3 and Example 1 is that the calcination temperature is 700°C.
[0084] The AZO targets obtained in Example 1 and Comparative Examples 1, 2 and 3 were tested, and the test results are shown in Table 1.
[0085] Table 1
[0086]
[0087] It can be seen that the resistivity of the AZO target obtained in Example 1 and the resistivity when sputtered on the surface of the copper foil are lower, indicating that the purity and density of the obtained target are higher.
[0088] In summary, the present invention specifically selects acrylamide and N-N'methylenebisacrylamide as monomers and cross-linking agents, and adjusts the process during target preparation, so as to obtain an AZO target with higher purity, higher density and better uniformity. The AZO target is sputtered on a copper foil as a decorative layer with good adhesion to the copper foil and very low thickness. The obtained polymer battery copper current collector can promote the uniform distribution of lithium ions on the foil surface without affecting the interface impedance.
[0089] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention specification, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a copper current collector for a polymer battery, characterized in that: The following steps are involved: S1, preparing a solution of zinc nitrate, aluminum nitrate, acrylamide and N-N'methylenebisacrylamide, adding an initiator to react to obtain a gel, and drying the gel to obtain an AZO precursor; S1 is specifically: S1.1, respectively preparing a zinc nitrate aqueous solution and an aluminum nitrate aqueous solution with zinc nitrate and aluminum nitrate, and mixing the two to obtain a zinc-aluminum nitrate mixed solution; the molar ratio of zinc to aluminum in the zinc-aluminum nitrate mixed solution is 1:100-10:100; S1.2, adding acrylamide and N-N'methylenebisacrylamide to the zinc nitrate aluminum mixed solution, stirring until the solution is clear, then adding an initiator, and completing the cross-linking reaction under heating conditions to obtain a gel; the mass ratio of acrylamide to N-N'methylenebisacrylamide is 15:1~20:1; S1.3, drying the gel to obtain an AZO precursor; S2. The AZO precursor is heated from room temperature to 350-450°C at 0.5-0.6 kPa for vacuum calcination, and then kept warm for 3-3.5 hours in an inert gas environment to obtain AZO powder, with a heating rate of 8-12°C / min; the AZO powder is mixed with anhydrous ethanol and ball milled, and then the ethanol is evaporated to prepare a target material embryo, and the target material embryo is placed in a vacuum hot pressing sintering furnace, and the vacuum pump is turned on to evacuate until the vacuum degree reaches 10 -1 Up to 10 -2 Pa, pressurized to 120MPa, sintering temperature of 1250℃~1300℃, heating rate of 8~12℃ / min, sintering time of 3~4h, and naturally cooled to room temperature after sintering to obtain AZO target; S3. Use AZO target material to perform sputtering coating on the surface of copper foil. After sputtering coating, an annealing step is also included. The annealing is specifically as follows: raise the temperature of the glass substrate to 300°C and keep it for 3 minutes, then wait for it to naturally drop to room temperature and then remove the substrate to obtain a polymer battery copper current collector.
2. The method for preparing a polymer battery copper current collector according to claim 1, characterized in that: The total mass of acrylamide and N-N'methylenebisacrylamide in S1.2 is 3-8% of the total mass of the zinc-aluminum nitrate mixed solution.
3. The method for preparing a copper current collector for a polymer battery according to claim 1, characterized in that: The heating condition in S1.2 is water bath heating, and the water bath temperature is 75~80℃.
4. The method for preparing a polymer battery copper current collector according to claim 1, characterized in that: The specific sputtering coating of S3 is as follows: the copper foil is pasted on the glass substrate, the distance between the AZO target and the glass substrate is controlled at 50~60mm, the temperature of the glass substrate is raised to 200℃; then vacuum is evacuated for sputtering.
5. A polymer battery copper current collector prepared according to the method for preparing a polymer battery copper current collector according to any one of claims 1 to 4.