COF material, COF-based heterogeneous structure catalyst, and preparation method and application thereof
By encapsulating metal nanoparticles with phosphoric acid functionalized COF materials and preparing COF-P-Pd heterostructure catalysts through a photoreduction process, the challenges of COF materials in catalyst preparation in the existing technology are solved, and high activity and stable catalytic effects are achieved. , suitable for efficient H2O2 synthesis and industrial catalysis.
Patent Information
- Application Number
- CN202410075919.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-01-18
AI Technical Summary
Existing technologies face challenges in developing methods for preparing universal and controllable particle size metal nanocatalytic materials, especially when using the pore structure characteristics of covalent organic framework (COF) materials to synthesize highly active and easily recyclable nanometal heterogeneous phases. Catalyst aspects.
Phosphoric acid functionalized COF materials are used to encapsulate metal nanoparticles, and COF materials are generated through the condensation reaction of aldehyde monomers and amino monomers, and COF-based heterostructure catalysts are prepared through phosphoric acid modification and photoreduction processes to ensure the stability and stability of metal nanoparticles. Dispersion.
A COF-P-Pd heterostructure catalyst with stable chemical properties, high catalytic activity, and high gas mass transfer efficiency has been achieved, which has excellent potential for H2O2 synthesis and industrial catalytic applications.
Smart Images

Figure CN117700770B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalytic material preparation, and in particular to a COF material, a COF-based heterogeneous structure catalyst, and a preparation method and application thereof. Background Art
[0002] Hydrogen peroxide (H2O2, commonly known as hydrogen peroxide) is an important industrial raw material and chemical product, widely used in bleaching, disinfection, semiconductor manufacturing and chemical synthesis. - The preparation of H2O2 by oxygen reduction reaction is safe, portable, green and energy-saving, and has attracted extensive attention from researchers in recent years. The core of this technology is to develop efficient, stable and low-cost photocatalysts.
[0003] Metal nanoparticles play an important role in heterogeneous photocatalytic reactions. A large number of studies have revealed that the formation of ohmic contact between metal nanoparticles and semiconductors promotes the separation of photogenerated carriers, thereby improving the reaction efficiency; at the same time, the microstructure and chemical composition of metal nanoparticles are also key factors affecting the transfer and storage capacity of photogenerated carriers. In photocatalytic hydrogen peroxide or organic synthesis, regulating the selectivity of the product may be more important than increasing the reaction rate.
[0004] Porous materials such as mesoporous silica, metal-organic frameworks, and covalent organic frameworks have high internal specific surface areas and have attracted widespread attention in the catalytic application of using them as dispersed carriers to prepare highly active and stable metal nanoparticles. Covalent organic frameworks (COFs) are crystalline porous polymers obtained by assembling monomers linked by designable covalent bonds. They are crystalline porous materials with periodic topological structures, strong chain segment rigidity, regular pores and active sites (P, N, O, etc.) coordinated with metals, and high stability. They can anchor metal ions through coordination. In addition, most COF materials are semiconductor materials, and loaded metal nanoparticles can be prepared through photoreduction processes to prepare efficient and durable catalytic materials. Therefore, COF materials have broader application prospects in the controllable preparation of ultrafine metal nanoparticles. How to use the pore structure characteristics of COFs to synthesize size-controlled, highly active, and easily recyclable nanometal heterogeneous catalysts deserves further exploration. In recent years, the application of COFs in the preparation of metal nanocatalysts has been reported, but the development of universal and particle size-controllable metal nanocatalytic materials preparation methods still faces many challenges. Summary of the invention
[0005] In order to solve the problems in the prior art, the present invention provides a COF material, a COF-based heterogeneous structure catalyst, and a preparation method and application thereof.
[0006] In a first aspect, the present invention provides a COF material, which includes a product generated by a condensation reaction of an aldehyde monomer and an amino monomer, wherein the aldehyde monomer is selected from the compound shown in formula I,
[0007]
[0008] In Formula I, R1 is selected from a single bond or a C1-C4 alkylene group, and R2 is selected from hydrogen, halogen or a C1-C4 alkyl group;
[0009] The amino monomer is selected from the compound shown in formula II,
[0010]
[0011] In Formula II, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and one of R3, R4, R5 and R6 is amino, and R7, R8, R9 and R 10 are independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and R7, R8, R9 and R 10 One of them is amino.
[0012] In some embodiments, R1 is selected from a single bond, methylene or ethylene. In some embodiments, R2 is selected from hydrogen, fluorine, chlorine, bromine, methyl or ethyl. In some embodiments, the compound shown in Formula I is tris(4-formylphenyl)amine.
[0013] In some embodiments, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and one of R3, R4, R5 and R6 is amino. 10 are independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and R7, R8, R9 and R 10 One of them is amino.
[0014] In some embodiments, the compound represented by Formula II is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0015] In some embodiments, the COF material includes the structural units shown below:
[0016]
[0017] In a second aspect, the present invention provides a phosphoric acid-modified COF material, which includes a COF material and a
[0018] Preferably, the COF material comprises a product generated by a condensation reaction of an aldehyde monomer and an amino monomer, wherein the aldehyde monomer is selected from the compound shown in Formula I,
[0019]
[0020] In Formula I, R1 is selected from a single bond or a C1-C4 alkylene group, and R2 is selected from hydrogen, halogen or a C1-C4 alkyl group;
[0021] The amino monomer is selected from the compound shown in formula II,
[0022]
[0023] In Formula II, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and one of R3, R4, R5 and R6 is amino, and R7, R8, R9 and R 10 are independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and R7, R8, R9 and R 10 One of them is amino.
[0024] In some embodiments, R1 is selected from a single bond, methylene or ethylene. In some embodiments, R2 is selected from hydrogen, fluorine, chlorine, bromine, methyl or ethyl.
[0025] In some embodiments, the compound represented by Formula I is tris(4-formylphenyl)amine.
[0026] In some embodiments, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and one of R3, R4, R5 and R6 is amino. 10 are independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and R7, R8, R9 and R 10 One of them is amino.
[0027] In some embodiments, the compound represented by Formula II is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0028] In some embodiments, the phosphoric acid-modified COF material includes the following structural units
[0029]
[0030]
[0031] In a third aspect, the present invention provides a COF-based heterostructure catalyst, which includes a phosphoric acid-modified COF material and metal nanoparticles encapsulated in the pores of the phosphoric acid-modified COF material.
[0032] The phosphoric acid modified COF material comprises a COF material and a
[0033] Preferably, the COF material comprises a product generated by a condensation reaction of an aldehyde monomer and an amino monomer, wherein the aldehyde monomer is selected from the compound shown in Formula I,
[0034]
[0035] In Formula I, R1 is selected from a single bond or a C1-C4 alkylene group, and R2 is selected from hydrogen, halogen or a C1-C4 alkyl group;
[0036] The amino monomer is selected from the compound shown in formula II,
[0037]
[0038] In Formula II, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and one of R3, R4, R5 and R6 is amino, and R7, R8, R9 and R 10 are independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and R7, R8, R9 and R 10 One of them is amino.
[0039] In some embodiments, R1 is selected from a single bond, methylene or ethylene. In some embodiments, R2 is selected from hydrogen, fluorine, chlorine, bromine, methyl or ethyl.
[0040] In some embodiments, the compound represented by Formula I is tris(4-formylphenyl)amine.
[0041] In some embodiments, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and one of R3, R4, R5 and R6 is amino. 10 are independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and R7, R8, R9 and R 10 One of them is amino.
[0042] In some embodiments, the compound represented by Formula II is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0043] In some embodiments, the phosphoric acid-modified COF material includes the following structural units
[0044]
[0045] The present invention uses phosphoric acid functionalized COF materials to encapsulate metal nanoparticles, which can stabilize, disperse and passivate the metal nanoparticles.
[0046] In some embodiments, the metal nanoparticles are selected from one or more of palladium nanoparticles, platinum nanoparticles, copper nanoparticles, and nickel nanoparticles.
[0047] In a fourth aspect, the present invention provides a method for preparing a phosphoric acid-modified COF material, comprising the following steps:
[0048] S1: allowing an aldehyde monomer and an amino monomer to undergo a condensation reaction in the presence of a first solvent and a catalyst to obtain a condensation reaction product, wherein the aldehyde monomer is selected from the compound shown in Formula I,
[0049] The aldehyde monomer is selected from the compound shown in formula I,
[0050]
[0051] In formula I, R1 is selected from a single bond or C1-C4 alkylene, and R2 is selected from hydrogen, halogen or C1-C4 alkyl
[0052] The amino monomer is selected from the compound shown in formula II,
[0053]
[0054] In Formula II, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and one of R3, R4, R5 and R6 is amino, and R7, R8, R9 and R 10 are independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and R7, R8, R9 and R 10 One of them is amino;
[0055] S2: mixing the first solution containing phosphite with the dispersion containing the condensation reaction product of step S1, and then performing a second reaction to obtain the phosphoric acid-modified COF material.
[0056] In some embodiments, R1 is selected from a single bond, methylene or ethylene. In some embodiments, R2 is selected from hydrogen, fluorine, chlorine, bromine, methyl or ethyl.
[0057] In some embodiments, the compound represented by Formula I is tris(4-formylphenyl)amine.
[0058] In some embodiments, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and one of R3, R4, R5 and R6 is amino. 10are independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and R7, R8, R9 and R 10 One of them is amino.
[0059] In some embodiments, the compound represented by Formula II is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0060] In some embodiments, in step S1, the molar ratio of the aldehyde monomer to the amino monomer is 1:(1.0-3.0), for example, 1:1.5, 1:2 or 1:2.5.
[0061] In some embodiments, in step S1, the first solvent includes o-dichlorobenzene and n-butanol. In some embodiments, the volume ratio of o-dichlorobenzene to n-butanol is 1:(0.5-2), for example, 1:1 or 1:1.5.
[0062] In some embodiments, in step S1, the catalyst is selected from a C1-C4 organic acid solution. In some embodiments, the catalyst is selected from an acetic acid solution, such as an acetic acid aqueous solution. In some embodiments, the concentration of the acetic acid solution is 3M-8M, such as 4M, 5M, 6M or 7M.
[0063] In some embodiments, in step S1, the temperature of the condensation reaction is 110°C-150°C, for example, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C or 145°C.
[0064] In some embodiments, in step S1, the condensation reaction time is 48 h-96 h, for example, 50 h, 56 h, 60 h, 66 h, 72 h, 78 h, 80 h, 84 h, 90 h or 92 h.
[0065] In some embodiments, the condensation reaction product of step S1 is a solid product after washing, for example, with acetonitrile, extraction, and drying.
[0066] In some embodiments, in step S2, the phosphite is selected from one or more of dimethyl phosphite, diethyl phosphite, diisopropyl phosphite and di-n-butyl phosphite.
[0067] In some embodiments, in step S2, the first solution further includes trimethylsilyl bromide.
[0068] In some embodiments, in step S2, the solvent of the first solution is selected from acetonitrile.
[0069] In some embodiments, in step S2, in the first solution, the concentration of the phosphite is 0.1 mol / L-0.5 mol / L, for example, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L or 0.45 mol / L.
[0070] In some embodiments, in step S2, the mass ratio of the molar amount of the phosphite to the condensation reaction product is 1mmol:(10-100)mg, such as 1mmol:20mg, 1mmol:30mg, 1mmol:40mg, 1mmol:50mg, 1mmol:60mg, 1mmol:70mg, 1mmol:80mg, 1mmol:90mg or any value therebetween. In some embodiments, the mass ratio of the molar amount of the phosphite to the condensation reaction product is 1mmol:(30-60)mg.
[0071] In some embodiments, in step S2, in the dispersion containing the condensation reaction product of step S1, the concentration of the condensation reaction product is 5 mol / L-50 mol / L, for example, 10 mol / L, 15 mol / L, 20 mol / L, 25 mol / L, 30 mol / L, 35 mol / L, 40 mol / L or 45 mol / L. In some embodiments, the solvent of the dispersion is selected from acetonitrile.
[0072] In some embodiments, in step S2, the temperature of the second reaction is 80°C-150°C, for example, 90°C, 100°C, 110°C, 120°C, 130°C or 140°C. In some embodiments, in step S2, the temperature of the second reaction is 100°C-120°C.
[0073] In some embodiments, in step S2, the time of the second reaction is 48 h-96 h, for example, 50 h, 56 h, 60 h, 66 h, 72 h, 78 h, 80 h, 84 h, 90 h or 92 h.
[0074] In some embodiments, a method for preparing a phosphoric acid-modified COF material comprises the following specific steps:
[0075] 1) Synthesis of COF nanosheets:
[0076] Take o-dichlorobenzene and n-butanol in a volume ratio of 1:1 respectively, mix them to obtain a first mixed solvent, add 0.04 mmol aldehyde monomer and 0.06 mmol amino monomer to 1 mL of the first mixed solvent, add the substrate into a pressure tube, and ultrasonicate for 60 seconds, then add 0.1 mL 6M acetic acid solution into the above system, and ultrasonicate for 10 seconds, vacuumize by rapid liquid nitrogen freeze-thaw cycle, and then stir the reaction at 120°C for 72 hours, wash with acetonitrile, extract with Soxhlet, and dry to obtain two-dimensional COF nanosheets (COF NS).
[0077] The aldehyde monomer is tri(4-formylphenyl)amine.
[0078] The amino monomer is 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0079] 2) Phosphoric acid functionalization of COF-P nanosheets:
[0080] 0.5mmol diethyl phosphite was added to 2mL anhydrous acetonitrile to obtain a first solution, 2mmol trimethylsilane bromide was slowly added dropwise to the first solution, and the mixed solution was stirred at room temperature for 2h. Subsequently, 30mg COF NS was dispersed in 2mL anhydrous acetonitrile, ultrasonicated for 1h to obtain a COF NS dispersion, and the COF NS dispersion was added dropwise to the above mixed solution, and the mixture was ultrasonicated for another 2h at room temperature. Then the tube was quickly frozen at 77K (liquid N2 bath), and degassed three times by freeze pump-thaw cycle, and the tube was sealed and stirred for 72h. The precipitate was washed three times by methanol centrifugation and dried in vacuo at 60℃ for 24h to obtain phosphoric acid functionalized COF nanosheets (COF-P NS).
[0081] In a fifth aspect, the present invention provides a method for preparing a COF-based heterostructure catalyst, comprising the following steps:
[0082] S3: allowing the phosphoric acid-modified COF material to undergo a third reaction with the second solution containing a metal source to obtain a phosphoric acid-modified COF material encapsulating metal ions;
[0083] S4: reducing the phosphoric acid-modified COF material encapsulating the metal ions to obtain the COF-based heterostructure catalyst;
[0084] Preferably, the method for preparing the phosphoric acid-modified COF material comprises the following steps:
[0085] S1: allowing an aldehyde monomer and an amino monomer to undergo a condensation reaction in the presence of a first solvent and a catalyst to obtain a condensation reaction product, wherein the aldehyde monomer is selected from the compound shown in Formula I,
[0086] The aldehyde monomer is selected from the compound shown in formula I,
[0087]
[0088] In formula I, R1 is selected from a single bond or C1-C4 alkylene, and R2 is selected from hydrogen, halogen or C1-C4 alkyl
[0089] The amino monomer is selected from the compound shown in formula II,
[0090]
[0091] In Formula II, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and one of R3, R4, R5 and R6 is amino, and R7, R8, R9 and R 10 are independently selected from hydrogen, amino, halogen or C1-C4 alkyl, and R7, R8, R9 and R 10 One of them is amino;
[0092] S2: mixing the first solution containing phosphite with the dispersion containing the condensation reaction product of step S1, and then performing a second reaction to obtain the phosphoric acid-modified COF material.
[0093] The present invention first synthesizes a catalyst having the ability to react with metal Pd 2+ The coordinated COF-P material combines metal Pd 2+ The ions are anchored to the COF-P nanosheets. Due to the semiconductor properties of COF-P, the Pd 2+ ions to prepare a COF-P-Pd heterostructure catalyst.
[0094] In some embodiments, R1 is selected from a single bond, methylene or ethylene. In some embodiments, R2 is selected from hydrogen, fluorine, chlorine, bromine, methyl or ethyl.
[0095] In some embodiments, the compound represented by Formula I is tris(4-formylphenyl)amine.
[0096] In some embodiments, R3, R4, R5 and R6 are each independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and one of R3, R4, R5 and R6 is amino. 10 are independently selected from hydrogen, amino, fluorine, chlorine, bromine, methyl or ethyl, and R7, R8, R9 and R 10 One of them is amino.
[0097] In some embodiments, the compound represented by Formula II is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0098] In some embodiments, in step S1, the molar ratio of the aldehyde monomer to the amino monomer is 1:(1.0-3.0), for example, 1:1.5, 1:2 or 1:2.5.
[0099] In some embodiments, in step S1, the first solvent includes o-dichlorobenzene and n-butanol. In some embodiments, the volume ratio of o-dichlorobenzene to n-butanol is 1:(0.5-2), for example, 1:1 or 1:1.5.
[0100] In some embodiments, in step S1, the catalyst is selected from a C1-C4 organic acid solution. In some embodiments, the catalyst is selected from an acetic acid solution, such as an acetic acid aqueous solution. In some embodiments, the concentration of the acetic acid solution is 3M-8M, such as 4M, 5M, 6M or 7M.
[0101] In some embodiments, in step S1, the temperature of the condensation reaction is 110°C-150°C, for example, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C or 145°C.
[0102] In some embodiments, in step S1, the condensation reaction time is 48 h-96 h, for example, 50 h, 56 h, 60 h, 66 h, 72 h, 78 h, 80 h, 84 h, 90 h or 92 h.
[0103] In some embodiments, the condensation reaction product of step S1 is a solid product after washing, for example, with acetonitrile, extraction, and drying.
[0104] In some embodiments, in step S2, the phosphite is selected from one or more of dimethyl phosphite, diethyl phosphite, diisopropyl phosphite and di-n-butyl phosphite.
[0105] In some embodiments, in step S2, the first solution further includes trimethylsilyl bromide.
[0106] In some embodiments, in step S2, the solvent of the first solution is selected from acetonitrile.
[0107] In some embodiments, in step S2, in the first solution, the concentration of the phosphite is 0.1 mol / L-0.5 mol / L, for example, 0.15 mol / L, 0.2 mol / L, 0.25 mol / L, 0.3 mol / L, 0.35 mol / L, 0.4 mol / L or 0.45 mol / L.
[0108] In some embodiments, in step S2, the mass ratio of the molar amount of the phosphite to the condensation reaction product is 1mmol:(10-100)mg, such as 1mmol:20mg, 1mmol:30mg, 1mmol:40mg, 1mmol:50mg, 1mmol:60mg, 1mmol:70mg, 1mmol:80mg, 1mmol:90mg or any value therebetween. In some embodiments, the mass ratio of the molar amount of the phosphite to the condensation reaction product is 1mmol:(30-60)mg.
[0109] In some embodiments, in step S2, in the dispersion containing the condensation reaction product of step S1, the concentration of the condensation reaction product is 5 mol / L-50 mol / L, for example, 10 mol / L, 15 mol / L, 20 mol / L, 25 mol / L, 30 mol / L, 35 mol / L, 40 mol / L or 45 mol / L. In some embodiments, the solvent of the dispersion is selected from acetonitrile.
[0110] In some embodiments, in step S2, the temperature of the second reaction is 80°C-150°C, for example, 90°C, 100°C, 110°C, 120°C, 130°C or 140°C. In some embodiments, in step S2, the temperature of the second reaction is 100°C-120°C.
[0111] In some embodiments, in step S2, the time of the second reaction is 48 h-96 h, for example, 50 h, 56 h, 60 h, 66 h, 72 h, 78 h, 80 h, 84 h, 90 h or 92 h.
[0112] In some embodiments, in step S3, the metal source is selected from one or more soluble metal salts. In some embodiments, in step S3, the metal source is selected from one or more of metal chlorides, metal sulfates, metal nitrates and metal acetates. In some embodiments, the metal source is selected from one or more of palladium chloride, palladium acetate, chloroplatinic acid, copper acetate and nickel acetate.
[0113] In some embodiments, the metal source is selected from one or more of palladium chloride, palladium sulfate, palladium nitrate, and palladium acetate.
[0114] In some embodiments, in step S3, the solvent of the second solution includes water and / or methanol. In some embodiments, the volume ratio of water to methanol is 0.1:(1-0.1).
[0115] In some embodiments, in step S3, the concentration of the metal source in the second solution is 0.0005 mol / mL-0.005 mol / mL, for example, 0.001 mol / mL, 0.002 mol / mL, 0.003 mol / mL or 0.004 mol / mL, calculated as the metal element.
[0116] In some embodiments, in step S3, the mass ratio of the molar amount of the metal source to the phosphoric acid modified COF material is 1 mmol: (0.5-15) mg, for example, 1 mmol: 1 mg, 2 mmol: 1 mg, 3 mmol: 1 mg, 4 mmol: 1 mg, 5 mmol: 1 mg, 6 mmol: 1 mg, 7 mmol: 1 mg, 8 mmol: 1 mg, 9 mmol: 1 mg, 10 mmol: 1 mg, 11 mmol: 1 mg, 12 mmol: 1 mg, 13 mmol: 1 mg, 14 mmol: 1 mg or any value therebetween. In some embodiments, the mass ratio of the molar amount of the metal source to the phosphoric acid modified COF material is 1 mmol: (1-10) mg.
[0117] In some embodiments, in step S3, the temperature of the third reaction is 60°C-120°C, for example, 70°C, 80°C, 90°C, 100°C or 110°C.
[0118] In some embodiments, in step S3, the time of the third reaction is 12 h-48 h, for example, 15 h, 20 h, 24 h, 36 h or 40 h.
[0119] In some embodiments, in step S4, the reduction is: mixing the phosphoric acid-modified COF material encapsulating the metal ions with an aqueous solution, and then performing photoreduction under irradiation of a light source.
[0120] In some embodiments, the light source is selected from a xenon lamp light source.
[0121] In some embodiments, the photoreduction time is 0.5 h-5 h, for example, 1 h, 2 h, 3 h or 4 h.
[0122] In some embodiments, the preparation method of the COF-based heterostructure catalyst comprises the following specific steps:
[0123] 1) Synthesis of COF nanosheets:
[0124] Take o-dichlorobenzene and n-butanol in a volume ratio of 1:1 respectively, mix them to obtain a first mixed solvent, add 0.04 mmol aldehyde monomer and 0.06 mmol amino monomer to 1 mL of the first mixed solvent, add the substrate into a pressure tube, and ultrasonicate for 60 seconds, then add 0.1 mL 6M acetic acid solution into the above system, and ultrasonicate for 10 seconds, vacuumize by rapid liquid nitrogen freeze-thaw cycle, and then stir the reaction at 120°C for 72 hours, wash with acetonitrile, extract with Soxhlet, and dry to obtain two-dimensional COF nanosheets (COF NS).
[0125] The aldehyde monomer is tri(4-formylphenyl)amine.
[0126] The amino monomer is 2,7-diaminocarbazole or 3,6-diaminocarbazole.
[0127] 2) Phosphoric acid functionalization of COF-P nanosheets:
[0128] 0.5mmol diethyl phosphite was added to 2mL anhydrous acetonitrile to obtain a first solution, 2mmol trimethylsilane bromide was slowly added dropwise to the first solution, and the mixed solution was stirred at room temperature for 2h. Subsequently, 30mg COF NS was dispersed in 2mL anhydrous acetonitrile, ultrasonicated for 1h to obtain a COF NS dispersion, and the COF NS dispersion was added dropwise to the above mixed solution, and the mixture was ultrasonicated for another 2h at room temperature. Then the tube was quickly frozen at 77K (liquid N2 bath), and degassed three times by freeze pump-thaw cycle, and the tube was sealed and stirred for 72h. The precipitate was washed three times by methanol centrifugation and dried in vacuo at 60℃ for 24h to obtain phosphoric acid functionalized COF nanosheets (COF-P NS).
[0129] 3) COF-P-Pd 2+ Preparation of composite materials:
[0130] Water and methanol were taken at a volume ratio of 0.1:1 to 0.1:1, respectively, and mixed to obtain a second solvent; palladium chloride was added to the solvent at a ratio of 0.01 to 0.10 mol of palladium chloride to 10 mL of the solvent, and magnetic stirring was performed until the palladium chloride was completely dissolved to obtain a mixed solution; then, COF-P nanosheets (COF-P NS) were added to the mixed solution at a ratio of 100 mg of COF-P nanosheets to 10 mL of the mixed solution, and the temperature was raised to 80°C for 24 hours to allow Pd 2+ The noble metal ion COF-P-Pd was anchored on COF-P NS by coordination, and the reactant was washed with solvent at least three times to obtain the noble metal ion COF-P-Pd 2+ Material;
[0131] 4) Preparation of COF-P-Pd heterostructure catalyst:
[0132] Add 100 mg COF-P-Pd into 10 mL deionized water. 2+ The ratio of materials, deionized water and COF-P-Pd 2+ Materials were added into a round bottom flask; COF-P-Pd 2+ The material was added to deionized water and ultrasonicated for 5 to 10 minutes to make it evenly dispersed. The round-bottom flask was then moved to a xenon lamp light source for photoreduction and magnetically stirred for 2 hours. The material was separated by suction, washed and dried to obtain a COF-P-Pd heterostructure catalyst.
[0133] In a sixth aspect, the present invention provides the use of the above-mentioned COF-based heterostructure catalyst or the COF-based heterostructure catalyst prepared by the above-mentioned preparation method in photocatalysis, especially photocatalytic production of hydrogen peroxide.
[0134] Compared with the prior art, the present invention has the following beneficial effects:
[0135] The preparation method of the present invention is to first synthesize a 2+ The coordinated COF-P material combines metal Pd 2+ The ions are anchored to the COF-P nanosheets. Due to the semiconductor properties of COF-P, the Pd 2+ Ions are used to prepare a COF-P-Pd heterostructure catalyst. The COF-P-Pd heterostructure catalyst obtained by the preparation method of the present invention has the characteristics of stable chemical properties, high catalytic activity, high gas mass transfer efficiency, and controllable noble metal particle size and morphology, and has very excellent application potential in the fields of efficient H2O2 synthesis and industrial catalysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0136] Figure 1 This is a physical picture of the COF-based (COF-P-Pd) heterostructure catalyst during the photoreduction process of Example 1 of the present invention.
[0137] Figure 2 It is an electron microscope image of the phosphoric acid modified COF material (COF-P) and the COF-based (COF-P-Pd) heterostructure catalyst of Example 1 of the present invention;
[0138] Among them, Figure a and Figure b are electron microscope images of COF-P materials, and Figure c is an electron microscope image of COF-P-Pd heterostructure catalyst.
[0139] Figure 3 3 is the XRD diagram of the COF nanosheet material (COF) of Example 1 of the present invention.
[0140] Figure 4Graph showing the catalytic performance of the COF-based (COF-P-Pd) heterostructure catalyst of Example 1 of the present invention and the COF-based (COF-P) heterostructure catalyst of Comparative Example 1. DETAILED DESCRIPTION
[0141] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments and drawings. The specific embodiments described herein are only used to explain the present invention and are not intended to constitute any limitation to the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concepts of the present disclosure. Such structures and technologies are also described in many publications.
[0142] Example 1
[0143] Step (1) Take o-dichlorobenzene and n-butanol in a volume ratio of 1:1, mix well, and obtain a first mixed solvent. Add 0.04mmol tris(4-formylphenyl)amine and 0.06mmol 3,6-diaminocarbazole to 1mL of the first mixed solvent, add the substrate into a pressure tube, and ultrasonicate for 60s. Then, add 0.1mL of 6M acetic acid solution to the above system, and ultrasonicate for 10s. Rapidly freeze-thaw cycle of liquid nitrogen to evacuate, then stir and react at 120°C for 72h, wash with acetonitrile, extract with Soxhlet, and dry to obtain a two-dimensional COF nanosheet (COF NS).
[0144] The specific reaction process is as follows:
[0145]
[0146] Step (2) 0.5 mmol of diethyl phosphite is added to 2 mL of anhydrous acetonitrile to obtain a first solution. 2 mmol of trimethylsilyl bromide is slowly added dropwise to the first solution to obtain a mixed solution, and the mixed solution is stirred at room temperature for 2 hours. Subsequently, 30 mg of COF NS is dispersed in 2 mL of anhydrous acetonitrile and ultrasonicated for 1 hour to obtain a COF NS dispersion. The COF NS dispersion is added dropwise to the above mixed solution, and the mixture is ultrasonicated for another 2 hours at room temperature. The tube is then quickly frozen at 77K (liquid N2 bath), and degassed three times by a freeze pump-thaw cycle. After the tube is sealed, it is stirred at 120°C for 72 hours, and the precipitate is washed three times by methanol centrifugation, and vacuum dried at 60°C for 24 hours to obtain phosphoric acid functionalized COF nanosheets (COF-P NS).
[0147] The specific reaction process is as follows:
[0148]
[0149] Step (3) Take water and methanol at a volume ratio of 1:1, mix them, and obtain a second solvent. Add palladium chloride to the second solvent at a ratio of 0.01 mol of palladium chloride to 10 mL of solvent, and stir magnetically until the palladium chloride is completely dissolved to obtain a mixed solution. Then, add COF-P nanosheets (COF-P NS) to the mixed solution at a ratio of 100 mg of COF-P nanosheets to 10 mL of the mixed solution, and heat to 80°C for 24 hours to allow Pd 2+ The noble metal ion COF-P-Pd was anchored on COF-P NS by coordination, and the reactant was washed with solvent at least three times to obtain the noble metal ion COF-P-Pd 2+ Material.
[0150] Step (4) Add 100 mg COF-P-Pd to 10 mL deionized water 2+ The ratio of materials, deionized water and COF-P-Pd 2+ The materials were added into a round bottom flask. COF-P-Pd 2+ The material was added to deionized water and ultrasonicated for 5 to 10 minutes to make it dispersed evenly. The round-bottom flask was then moved to a xenon lamp light source for photoreduction and magnetically stirred for 2 hours. The COF-P-Pd heterostructure catalyst was obtained by filtration, washing and drying. Figure 1 It can be seen that COF-P-Pd 2+ The dispersion was yellow, and after photoreduction, the color of the dispersion changed to deep orange-red due to the formation of Pd nanoparticles and the preparation of COF-P-Pd.
[0151] The electron microscopy images of the phosphoric acid functionalized COF material (COF-P) and the COF-P-Pd heterostructure catalyst prepared in this example are as follows: Figure 2 As shown. Figure 2 a and Figure 2 b It can be seen that COF-P presents a nanosheet structure. After photoreduction, Figure 2 c The generation of Pd nanoparticles on COF-P nanosheets can be seen.
[0152] The XRD pattern of the COF nanosheet material (COF) prepared in this example is as follows: Figure 3 shown.
[0153] Example 2
[0154] Step (1) Take o-dichlorobenzene and n-butanol in a volume ratio of 1:1, mix them, and obtain a first mixed solvent. Add 0.04mmol tris(4-formylphenyl)amine and 0.06mmol 2,7-diaminocarbazole to 1mL of the first mixed solvent, add the substrate into a pressure tube, and ultrasonicate for 60s. Then, add 0.1mL of 6M acetic acid solution to the above system, ultrasonicate for 10s, quickly freeze-thaw and cycle liquid nitrogen to evacuate, and then stir and react at 120°C for 72h, wash with acetonitrile, extract with Soxhlet, and dry to obtain a two-dimensional COF nanosheet (COF NS).
[0155] The specific reaction process is as follows:
[0156]
[0157] Step (2) 0.5 mmol of diethyl phosphite is added to 2 mL of anhydrous acetonitrile to obtain a first solution. 2 mmol of trimethylsilyl bromide is slowly added dropwise to the first solution to obtain a mixed solution, and the mixed solution is stirred at room temperature for 2 hours. Subsequently, 30 mg of COF NS is dispersed in 2 mL of anhydrous acetonitrile and ultrasonicated for 1 hour to obtain a COF NS dispersion. The COF NS dispersion is added dropwise to the above mixed solution, and the mixture is ultrasonicated for another 2 hours at room temperature. The tube is then quickly frozen at 77K (liquid N2 bath), and degassed three times by a freeze pump-thaw cycle. After the tube is sealed, it is stirred at 120°C for 72 hours, and the precipitate is washed three times by methanol centrifugation, and vacuum dried at 60°C for 24 hours to obtain phosphoric acid functionalized COF nanosheets (COF-P NS).
[0158] The specific reaction process is as follows:
[0159]
[0160] Step (3) Take water and methanol at a volume ratio of 0.1 to 0.1:1, mix well, and obtain a second solvent. Add palladium chloride to the second solvent at a ratio of 0.10 mol of palladium chloride to 10 mL of solvent, and stir magnetically until the palladium chloride is completely dissolved to obtain a mixed solution. Then, add COF-P nanosheets (COF-P NS) to the mixed solution at a ratio of 100 mg of COF-P nanosheets to 10 mL of the mixed solution, heat to 80°C and react for 24 hours to allow Pd 2+ The noble metal ion COF-P-Pd was anchored on COF-P NS by coordination, and the reactant was washed with solvent at least three times to obtain the noble metal ion COF-P-Pd 2+ Material.
[0161] Step (4) Add 100 mg COF-P-Pd to 10 mL deionized water 2+ The ratio of materials, deionized water and COF-P-Pd2+ The materials were added into a round bottom flask. COF-P-Pd 2+ The material was added to deionized water and ultrasonicated for 5 to 10 minutes to make it dispersed evenly. The round-bottom flask was then moved to a xenon lamp light source for photoreduction and magnetically stirred for 2 hours. The material was separated by suction, washed and dried to obtain a COF-P-Pd heterostructure catalyst.
[0162] Comparative Example 1
[0163] The phosphoric acid functionalized COF nanosheets (COF-P NS) prepared in Example 1 were used as the COF-P heterostructure catalyst of Comparative Example 1.
[0164] Performance Testing
[0165] The photocatalytic hydrogen peroxide production performance test was carried out using the catalysts prepared in Example 1 and Comparative Example 1. Specifically, the catalyst material and deionized water were prepared into a 1 mg / mL suspension, and then 10 mL was extracted for catalytic reaction under a xenon light source. Test results Figure 4 As shown in the figure, it can be seen that the metal nanoparticle catalyst encapsulated by the phosphoric acid functionalized COF material has higher catalytic activity.
[0166] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A COF material comprising a product generated by a condensation reaction of an aldehyde monomer and an amino monomer, wherein: The aldehyde monomer is selected from tris(4-formylphenyl)amine, and the amino monomer is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole.
2. The COF material according to claim 1, characterized in that: The COF material includes the following structural units:
3. A phosphoric acid-modified COF material, comprising the COF material according to claim 1 or 2 and a 4. The phosphoric acid-modified COF material according to claim 3, characterized in that: The phosphoric acid-modified COF material includes the following structural units:
5. A COF-based heterostructure catalyst, comprising the phosphoric acid-modified COF material according to claim 3 or 4 and metal nanoparticles encapsulated in the pores of the phosphoric acid-modified COF material, wherein the metal nanoparticles are selected from one or more of palladium nanoparticles, platinum nanoparticles, copper nanoparticles and nickel nanoparticles.
6. A method for preparing a phosphoric acid-modified COF material, comprising the following steps: S1: allowing an aldehyde monomer and an amino monomer to undergo a condensation reaction in the presence of a first solvent and a catalyst to obtain a condensation reaction product, wherein the aldehyde monomer is tris(4-formylphenyl)amine, The amino monomer is selected from 2,7-diaminocarbazole or 3,6-diaminocarbazole; S2: mixing the first solution containing phosphite with the dispersion containing the condensation reaction product of step S1, and then performing a second reaction to obtain the phosphoric acid-modified COF material.
7. The preparation method according to claim 6, characterized in that: In step S1, the molar ratio of the aldehyde monomer to the amino monomer is 1:(1.0-3.0); and / or In step S1, the first solvent includes o-dichlorobenzene and n-butanol; and / or In step S1, the catalyst is selected from a C1-C4 organic acid solution; and / or In step S1, the temperature of the condensation reaction is 110°C-150°C, and the time of the condensation reaction is 48h-96h.
8. The preparation method according to claim 7, characterized in that: The volume ratio of o-dichlorobenzene to n-butanol is 1:(0.5-2); and / or The catalyst is selected from acetic acid solution.
9. The preparation method according to any one of claims 6 to 8, characterized in that: In step S2, the phosphite is selected from one or more of dimethyl phosphite, diethyl phosphite, diisopropyl phosphite and di-n-butyl phosphite; and / or In step S2, the first solution further comprises trimethylsilyl bromide; the solvent of the first solution is selected from acetonitrile; and / or In step S2, the mass ratio of the molar amount of the phosphite to the condensation reaction product is 1 mmol: (10-100) mg; and / or In step S2, the temperature of the second reaction is 80°C-150°C, and the time of the second reaction is 48h-96h.
10. The preparation method according to claim 9, characterized in that: The mass ratio of the molar amount of the phosphite to the condensation reaction product is 1 mmol: (30-60) mg; and / or The temperature of the second reaction is 100°C-120°C.
11. A method for preparing a COF-based heterogeneous structure catalyst, comprising the following steps: S3: allowing the phosphoric acid-modified COF material to undergo a third reaction with the second solution containing a metal source to obtain a phosphoric acid-modified COF material encapsulating metal ions, wherein the phosphoric acid-modified COF material is selected from the phosphoric acid-modified COF material according to claim 3 or 4 or the phosphoric acid-modified COF material prepared by the preparation method according to any one of claims 6 to 10, and the metal source is selected from one or more of palladium chloride, palladium acetate, chloroplatinic acid, copper acetate and nickel acetate; S4: reducing the phosphoric acid-modified COF material encapsulating the metal ions to obtain the COF-based heterostructure catalyst.
12. The preparation method according to claim 11, characterized in that: In step S3 The solvent of the second solution includes water and / or methanol; and / or The mass ratio of the molar amount of the metal source to the phosphoric acid-modified COF material is 1 mmol: (0.5-15) mg, calculated as the metal element; and / or The temperature of the third reaction is 60° C.-120° C., and the time of the third reaction is 12 h-48 h.
13. The preparation method according to claim 12, characterized in that: The volume ratio of water to methanol is 0.1:(1-0.1); and / or The mass ratio of the molar amount of the metal source to the phosphoric acid-modified COF material is 1 mmol:(1-10) mg.
14. The preparation method according to any one of claims 11 to 13, characterized in that: In step S4, the reduction is: mixing the phosphoric acid-modified COF material encapsulating the metal ions with an aqueous solution, and then performing photoreduction under irradiation of a light source.
15. The preparation method according to claim 14, characterized in that: The light source is selected from a xenon lamp light source.
16. The preparation method according to claim 14, characterized in that: The photoreduction time is 0.5h-5h.
17. Use of the COF-based heterostructure catalyst according to claim 5 or the COF-based heterostructure catalyst obtained by the preparation method of any one of claims 11 to 16 in photocatalytic production of hydrogen peroxide.
Citation Information
Patent Citations
Gold-doped covalent organic framework material and preparation method and application thereof, covalent organic framework nano-enzyme biological probe and application thereof, and kit
CN114577746A
Covalent organic framework material based on benzodifuran diketone as well as preparation method and application of covalent organic framework material
CN117384333A