A process for preparing manganese-vanadium microalloy high-strength steel

Through the preparation process of manganese-vanadium micro-alloyed high-strength steel, using scrap steel resources, combined with heat treatment, ion implantation, plasma technology and rapid cooling, the problems of uniformity of alloy elements and structural stability are solved, and the strength and hardness of the steel are improved, achieving Efficient resource utilization and environmentally friendly preparation of high-strength steel.

CN117701982BActive Publication Date: 2024-10-01SHANDONG IRON & STEEL GRP YONGFENG LINGANG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311509157.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-14
Publication Date
2024-10-01
Estimated Expiration
2043-11-14

AI Technical Summary

Technical Problem

In traditional high-strength steel preparation methods, it is difficult to control the uniformity of alloy elements and structural stability, resulting in inconsistent products, and it is difficult to achieve uniform distribution and content control of nitrogen elements.

Method used

The manufacturing process of manganese-vanadium microalloy high-strength steel is adopted, by selecting scrap steel containing manganese and vanadium as raw materials, performing heat treatment and oxidation reduction, introducing trace alloy elements and using ion implantation or plasma technology, combined with high-temperature smelting and rapid cooling technology. To ensure the uniformity of the alloy composition and the stability of the structural structure, water quenching and heat treatment are used to adjust the structural structure, and trace amounts of nitrogen and graphite covering agents are introduced during the smelting process.

Benefits of technology

It achieves uniform distribution of alloying elements and stability of the organizational structure, improves the strength and performance of steel, reduces dependence on original ore, reduces environmental burden, and improves preparation effects and finished product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention relates to the technical field of alloy high-strength steel preparation, and discloses a method for preparing manganese-vanadium microalloy high-strength steel, which comprises the following steps: Step 1, selecting scrap steel containing manganese and vanadium as the original alloy material, wherein the other alloy elements contained in the scrap steel include chromium and molybdenum, and the contents are 0.3-0.7% chromium and 0.1-0.5% molybdenum respectively; Step 2, performing pretreatment in the raw material, including heat treatment and oxidation-reduction steps, wherein the heat treatment heats the material to 800-1000°C and keeps it at this temperature for 1-3 hours, and during the oxidation-reduction process, a reducing agent is used to reduce the oxide content to 0.07-0.1%; Step 3, introducing trace alloy elements. By controlling the alloy element content and introducing trace alloy elements, adjusting the alloy structure, improving the strength and performance of the steel, and further optimizing the structure through water quenching and heat treatment processes, enhancing the strength and hardness of the steel, it is helpful to improve the preparation effect and quality of the alloy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy high-strength steel preparation, and in particular to a process for preparing manganese-vanadium microalloy high-strength steel. Background Art

[0002] The material of the steel reinforcement rod used in construction is alloy material, which is mainly used for active reinforcement of mines, slopes, tunnels, dams and other projects. In the past ten years, the ultimate bearing capacity, length and concentration of anchoring force of the reinforcement rod have all shown a steady growth trend. With the rise of high-rise and super-high-rise buildings, the construction of spearheads, tunnels and dams, the application of reinforcement rods has become more and more extensive, and the market demand for high-strength reinforcement rods has increased. In order to improve the stability of engineering structures, high-strength reinforcement rods have put forward new requirements for production processes.

[0003] In traditional high-strength steel preparation methods, the uniformity of alloying elements and the stability of the organizational structure are often challenged, which may lead to inconsistency in products. Although the technology of introducing nitrogen elements helps to improve the nitriding strengthening effect, the current methods still have room for improvement in achieving uniform distribution of nitrogen elements and controlling the content. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a process for preparing manganese-vanadium microalloy high-strength steel, which solves the problem that there is still room for improvement in controlling the content in the current process of preparing high-strength steel.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A process for preparing manganese-vanadium microalloy high-strength steel, comprising the following steps;

[0006] Step 1: Selecting scrap steel containing manganese and vanadium as the original alloy material, wherein other alloy elements contained in the scrap steel include chromium and molybdenum, and the contents of the scrap steel are 0.3-0.7% chromium and 0.1-0.5% molybdenum respectively;

[0007] Step 2: pre-treating the raw material, including heat treatment and oxidation-reduction steps, wherein the heat treatment heats the material to 800-1000° C. and maintains the temperature for 1-3 hours, and during the oxidation-reduction process, a reducing agent is used to reduce the oxide content to 0.07-0.1%;

[0008] Step 3: Introduce trace alloying elements, use ion implantation technology or plasma technology to evenly distribute the trace elements Ti and Nb, and control the contents of manganese and vanadium to between 0.5-2% and 0.1-0.5%, respectively;

[0009] Step 4: Perform high-temperature smelting in an electric arc furnace or induction furnace, and ensure the uniformity and stability of the alloy structure through real-time monitoring of alloy composition and adaptive control technology;

[0010] Step 5: Use rapid cooling technology, water quenching, and subsequent heat treatment process to adjust the organizational structure of the manganese-vanadium microalloy high-strength steel, wherein the water quenching rate is controlled at 5 to 20°C / s.

[0011] Preferably, in step 1, other alloy elements contained in the original alloy material of scrap steel include nickel, with a content of 0.1 to 0.4%.

[0012] Preferably, in step three, the trace alloying elements of ion implantation technology or plasma technology include vanadium, niobium and titanium, and the contents thereof are 0.05-0.2%, 0.01-0.1% and 0.01-0.1%, respectively.

[0013] Preferably, in step 2, the oxidation-reduction step in the heat treatment process uses a reducing agent including hydrogen or carbon.

[0014] Preferably, in step 4, the temperature during the high-temperature smelting process is maintained between 1600 and 1800° C. for 1 to 2 hours.

[0015] Preferably, in step five, the heat treatment process after rapid cooling includes heating to 1000-1200° C. and holding time of 1-4 hours.

[0016] Preferably, in step five, the water quenching rate varies with temperature in a nonlinear manner, that is, as the temperature decreases, the water quenching rate gradually decreases.

[0017] Preferably, in step 4, a graphite covering agent is used in smelting.

[0018] Preferably, in step 4, a trace amount of nitrogen is introduced during the smelting process to control the content of nitrogen to 0.005-0.02%.

[0019] Preferably, in step 4, the slag needs to be cleaned regularly during the smelting process.

[0020] The present invention provides a method for preparing manganese-vanadium microalloy high-strength steel. It has the following beneficial effects:

[0021] The present invention utilizes scrap steel resources by selecting scrap steel containing manganese and vanadium as the original alloy material, and realizes the effective utilization of other alloy elements in the preparation process. By introducing the uniform distribution of trace alloy elements and controlling the contents of elements such as manganese, vanadium, titanium, and niobium, it is helpful to adjust the organizational structure of the alloy and improve the strength and performance of the steel. The use of water quenching and subsequent heat treatment processes is helpful to adjust the organizational structure of manganese-vanadium microalloy high-strength steel and further improve the strength and hardness of the steel. Measures such as maintaining temperature, applying graphite covering agents, introducing trace nitrogen elements, and regularly cleaning slag materials are all helpful to improve the preparation effect and quality of the alloy. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] Embodiment 1:

[0024] The embodiment of the present invention provides a method for preparing manganese-vanadium microalloy high-strength steel, comprising the following steps:

[0025] Step 1, selecting scrap steel containing manganese and vanadium as the original alloy material, the other alloy elements contained in the scrap steel include chromium and molybdenum, and the content of chromium is 0.5%, and the content of molybdenum is 0.3%, and the other alloy elements contained in the original alloy material of the scrap steel include nickel, and the content is 0.2%. Through the reuse of this scrap steel, the comprehensive utilization of resources is achieved, which helps to reduce the dependence on the original ore and reduce the environmental burden;

[0026] Step 2: Pretreatment is performed in the raw materials, including heat treatment and oxidation-reduction steps, wherein the heat treatment heats the material to 890°C and maintains it at this temperature for 2 hours. During the oxidation-reduction process, a reducing agent is used to reduce the oxide content to 0.09%. The heat treatment and oxidation-reduction steps performed in the raw materials help to purify the original alloy material and eliminate undesirable impurities and oxides, which helps to improve the purity of the alloy and provide more favorable conditions for subsequent processes;

[0027] Step 3: Introduce trace alloying elements, use ion implantation technology or plasma technology to evenly distribute the trace elements Ti and Nb, and control the contents of manganese and vanadium between 1.6% and 0.4%, respectively. The trace alloying elements of ion implantation technology or plasma technology include vanadium, niobium, and titanium, with contents of 0.13%, 0.08%, and 0.07%, respectively. The oxidation-reduction step in the heat treatment process uses a reducing agent, including hydrogen or carbon, to achieve uniform distribution of these elements, which helps to form a strengthening phase in the grain boundary and precipitated phase, thereby improving the performance of high-strength steel.

[0028] Step 4: High-temperature smelting is performed in an electric arc furnace or an induction furnace. The alloy composition is monitored in real time and adaptive control technology is used to ensure the uniformity and stability of the alloy structure. The temperature during high-temperature smelting is maintained between 1650°C and the time is 1.5 hours to ensure the uniformity and stability of the alloy structure. A graphite covering agent is used in the smelting process. A trace amount of nitrogen is introduced during the smelting process to control its content at 0.01%. The slag needs to be cleaned regularly during the smelting process, which further optimizes the smelting process of the alloy and helps to improve the quality of the finished product.

[0029] Step 5. Use rapid cooling technology, water quenching, and subsequent heat treatment process to adjust the microstructure of the manganese-vanadium microalloy high-strength steel, wherein the water quenching rate is controlled at 13°C / s, and the heat treatment process after rapid cooling includes heating to 1100°C and holding time for 3 hours. The water quenching rate changes with temperature in a nonlinear manner, that is, as the temperature decreases, the water quenching rate gradually decreases, which helps to adjust the microstructure of the manganese-vanadium microalloy high-strength steel. The nonlinear adjustment of the water quenching rate enables an ideal cooling effect to be obtained at different temperatures, thereby further improving the strength and toughness of the material.

[0030] According to the steps of Example 1, high-strength steel was prepared, and various performances of the finished product were tested, and the performance data of various aspects were recorded in Table 1.

[0031] Embodiment 2:

[0032] The embodiment of the present invention provides a method for preparing manganese-vanadium microalloy high-strength steel, comprising the following steps:

[0033] Step 1, selecting scrap steel containing manganese and vanadium as the original alloy material, the other alloy elements contained in the scrap steel include chromium and molybdenum, and the content of chromium is 0.5%, and the content of molybdenum is 0.3%, and the other alloy elements contained in the original alloy material of the scrap steel include nickel, and the content is 0.2%. Through the reuse of this scrap steel, the comprehensive utilization of resources is achieved, which helps to reduce the dependence on the original ore and reduce the environmental burden;

[0034] Step 2: Pretreatment is performed in the raw materials, including heat treatment and oxidation-reduction steps, wherein the heat treatment heats the material to 890°C and maintains it at this temperature for 2 hours. During the oxidation-reduction process, a reducing agent is used to reduce the oxide content to 0.07%. The heat treatment and oxidation-reduction steps performed in the raw materials help to purify the original alloy material and eliminate undesirable impurities and oxides, which helps to improve the purity of the alloy and provide more favorable conditions for subsequent processes;

[0035] Step 3: Introduce trace alloying elements, use ion implantation technology or plasma technology to evenly distribute the trace elements Ti and Nb, and control the contents of manganese and vanadium between 1.6% and 0.4%, respectively. The trace alloying elements of ion implantation technology or plasma technology include vanadium, niobium, and titanium, with contents of 0.13%, 0.08%, and 0.07%, respectively. The oxidation-reduction step in the heat treatment process uses a reducing agent, including hydrogen or carbon, to achieve uniform distribution of these elements, which helps to form a strengthening phase in the grain boundary and precipitated phase, thereby improving the performance of high-strength steel.

[0036] Step 4: High-temperature smelting is performed in an electric arc furnace or an induction furnace. The alloy composition is monitored in real time and adaptive control technology is used to ensure the uniformity and stability of the alloy structure. The temperature during high-temperature smelting is maintained between 1650°C and the time is 1.5 hours to ensure the uniformity and stability of the alloy structure. A graphite covering agent is used in the smelting process. A trace amount of nitrogen is introduced during the smelting process to control its content at 0.01%. The slag needs to be cleaned regularly during the smelting process, which further optimizes the smelting process of the alloy and helps to improve the quality of the finished product.

[0037] Step 5. Use rapid cooling technology, water quenching, and subsequent heat treatment process to adjust the microstructure of the manganese-vanadium microalloy high-strength steel, wherein the water quenching rate is controlled at 13°C / s, and the heat treatment process after rapid cooling includes heating to 1100°C and holding time for 3 hours. The water quenching rate changes with temperature in a nonlinear manner, that is, as the temperature decreases, the water quenching rate gradually decreases, which helps to adjust the microstructure of the manganese-vanadium microalloy high-strength steel. The nonlinear adjustment of the water quenching rate enables an ideal cooling effect to be obtained at different temperatures, thereby further improving the strength and toughness of the material.

[0038] According to the steps of Example 2, high-strength steel was prepared, and various performances of the finished product were tested, and the performance data of various aspects were recorded in Table 1.

[0039] Embodiment three:

[0040] The embodiment of the present invention provides a method for preparing manganese-vanadium microalloy high-strength steel, comprising the following steps:

[0041] Step 1, selecting scrap steel containing manganese and vanadium as the original alloy material, the other alloy elements contained in the scrap steel include chromium and molybdenum, and the content of chromium is 0.5%, and the content of molybdenum is 0.3%, and the other alloy elements contained in the original alloy material of the scrap steel include nickel, and the content is 0.2%. Through the reuse of this scrap steel, the comprehensive utilization of resources is achieved, which helps to reduce the dependence on the original ore and reduce the environmental burden;

[0042] Step 2: Pretreatment is performed in the raw materials, including heat treatment and oxidation-reduction steps, wherein the heat treatment heats the material to 890°C and maintains it at this temperature for 2 hours. During the oxidation-reduction process, a reducing agent is used to reduce the oxide content to 0.1%. The heat treatment and oxidation-reduction steps performed in the raw materials help to purify the original alloy material and eliminate undesirable impurities and oxides, which helps to improve the purity of the alloy and provide more favorable conditions for subsequent processes;

[0043] Step 3: Introduce trace alloying elements, use ion implantation technology or plasma technology to evenly distribute the trace elements Ti and Nb, and control the contents of manganese and vanadium between 1.6% and 0.4%, respectively. The trace alloying elements of ion implantation technology or plasma technology include vanadium, niobium, and titanium, with contents of 0.13%, 0.08%, and 0.07%, respectively. The oxidation-reduction step in the heat treatment process uses a reducing agent, including hydrogen or carbon, to achieve uniform distribution of these elements, which helps to form a strengthening phase in the grain boundary and precipitated phase, thereby improving the performance of high-strength steel.

[0044] Step 4: High-temperature smelting is performed in an electric arc furnace or an induction furnace. The alloy composition is monitored in real time and adaptive control technology is used to ensure the uniformity and stability of the alloy structure. The temperature during high-temperature smelting is maintained between 1650°C and the time is 1.5 hours to ensure the uniformity and stability of the alloy structure. A graphite covering agent is used in the smelting process. A trace amount of nitrogen is introduced during the smelting process to control its content at 0.01%. The slag needs to be cleaned regularly during the smelting process, which further optimizes the smelting process of the alloy and helps to improve the quality of the finished product.

[0045] Step 5. Use rapid cooling technology, water quenching, and subsequent heat treatment process to adjust the microstructure of the manganese-vanadium microalloy high-strength steel, wherein the water quenching rate is controlled at 13°C / s, and the heat treatment process after rapid cooling includes heating to 1100°C and holding time for 3 hours. The water quenching rate changes with temperature in a nonlinear manner, that is, as the temperature decreases, the water quenching rate gradually decreases, which helps to adjust the microstructure of the manganese-vanadium microalloy high-strength steel. The nonlinear adjustment of the water quenching rate enables an ideal cooling effect to be obtained at different temperatures, thereby further improving the strength and toughness of the material.

[0046] According to the steps of Example 3, high-strength steel was prepared, and various performances of the finished product were tested, and the performance data of various aspects were recorded in Table 1.

[0047]

[0048] Table 1

[0049] In summary, scrap steel containing manganese and vanadium is selected as the original alloy material, scrap steel resources are utilized, and other alloy elements are effectively utilized in the preparation process. The introduction of uniform distribution of trace alloying elements and control of the content of elements such as manganese, vanadium, titanium, and niobium help to adjust the microstructure of the alloy and improve the strength and performance of the steel. The use of water quenching and subsequent heat treatment processes helps to adjust the microstructure of manganese-vanadium microalloyed high-strength steel and further improve the strength and hardness of the steel. Temperature maintenance, the application of graphite covering agents, the introduction of trace nitrogen elements, and regular cleaning of slag are all helpful to improve the preparation effect and quality of the alloy.

[0050] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing manganese-vanadium microalloy high-strength steel, characterized in that: The steps include: Step 1: Select scrap steel containing manganese and vanadium as the original alloy material. The other alloy elements contained in the scrap steel include chromium and molybdenum, and the contents are 0.3-0.7% chromium and 0.1-0.5% molybdenum respectively. The other alloy elements contained in the original alloy material of the scrap steel include nickel, and the content is 0.1-0.4%; Step 2: pretreating the raw materials, including heat treatment and oxidation-reduction steps, wherein the heat treatment heats the materials to 800-1000°C and maintains the temperature for 1-3 hours, and during the oxidation-reduction process, a reducing agent is used to reduce the oxide content to 0.07-0.1%, and the oxidation-reduction step in the heat treatment process uses a reducing agent, including hydrogen or carbon; Step 3: Introduce trace alloying elements, use ion implantation technology to evenly distribute the trace elements Ti and Nb, and control the contents of manganese and vanadium to between 0.5-2% and 0.1-0.5%, respectively. The trace alloying elements of ion implantation technology include vanadium, niobium, and titanium, and their contents are 0.05-0.2%, 0.01-0.1%, and 0.01-0.1%, respectively. Step 4: Perform high-temperature smelting in an electric arc furnace or induction furnace. Real-time monitoring of alloy composition and adaptive control technology are used to ensure uniformity and stability of the alloy structure. The temperature during high-temperature smelting is maintained between 1600 and 1800°C for 1 to 2 hours. A trace amount of nitrogen is introduced during the smelting process to control its content between 0.005 and 0.02%. Step 5: Use rapid cooling technology, water quenching, and subsequent heat treatment process to adjust the organizational structure of the manganese-vanadium microalloy high-strength steel, wherein the water quenching rate is controlled at 5-20°C / s, and the heat treatment process after rapid cooling includes heating to 1000-1200°C and holding time for 1-4h.

2. The method for preparing a manganese-vanadium microalloyed high-strength steel according to claim 1, characterized in that: In the step 5, the water quenching rate changes with the temperature in a nonlinear manner, that is, as the temperature decreases, the water quenching rate gradually decreases.

3. The method for preparing a manganese-vanadium microalloyed high-strength steel according to claim 1, characterized in that: In the step 4, a graphite covering agent is used in the smelting.

4. The method for preparing a manganese-vanadium microalloyed high-strength steel according to claim 1, characterized in that: In the step 4, the slag needs to be cleaned regularly during the smelting process.