Continuous wave perovskite polariton laser and laser chip and manufacturing method
By introducing perovskite gain medium into the optical microcavity and adjusting the cavity mode, the implementation problem of perovskite polarized exciter laser in the continuous wave pump mode is solved, and a low threshold continuous coherent light source is realized, which improves the excitation Sub-life and laser device performance.
Patent Information
- Application Number
- CN202311741014.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-18
Smart Images

Figure CN117712823B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optoelectronic devices, and in particular to a low-threshold perovskite polariton laser and a laser chip that can operate in a continuous pumping mode, and a manufacturing method thereof. Background Art
[0002] When the coupling intensity between the excitons in the semiconductor and the cavity photons confined by the optical microcavity is greater than the attenuation of the excitons and cavity photons, a hybrid quasiparticle - exciton polaritons can be formed between them. This polariton is formed by the interaction between excitons and photons, and appears as a hybrid state of half light and half matter. When the density reaches a certain level, as the polaritons scatter each other and release phonons, they condense to the lowest quantum energy state, and the photon components leak out of the optical microcavity, forming a polariton laser. Compared with traditional semiconductor lasers, polariton lasers do not require population inversion to be realized, so in theory, their threshold is 1-2 orders of magnitude lower than that of photon lasers, which is more conducive to the generation of continuous wave lasers.
[0003] In the selection of polariton laser gain media, inorganic semiconductors have high dielectric constants and low hole effective masses, and their exciton binding energy is small, generally less than or approximately equal to 10 meV. They are easily thermally decomposed into free electron-hole pairs at room temperature, resulting in the phenomenon of exciton-polariton condensation being generally observed only at lower temperatures. For example, the temperature at which GaAs and CdTe achieve polariton condensation is around ~10K, which greatly limits the development and application of exciton-polaritons. In contrast, most of the exciton types in organic materials are Frenkel excitons, which have very weak dielectric shielding. Therefore, the excitons in organic materials often have large binding energies, usually hundreds of meV, and also have large oscillator strengths, and the critical temperature at which exciton-polaritons condensation can be observed is higher. However, the weak nonlinear effects and structural inhomogeneities of organic materials limit the spatial range and lifetime of exciton-polaritons. The Coulomb interaction between localized Frenkel excitons is weak, resulting in the weakening of the scattering effect between polaritons, which retards the condensation of exciton-polaritons. Therefore, polariton lasing in organic materials often has a larger threshold, sometimes even larger than the threshold of stimulated emission lasing relying on population inversion.
[0004] Metal halide perovskites have excellent optoelectronic properties. They can be prepared by solution method, have low crystallization temperature, are easy to process and are low in cost. These advantages make them one of the most popular luminescent and energy conversion materials, and they have been widely used in fields such as LEDs and solar cells. However, the field of perovskite lasers is still relatively low, especially in the direction of polaritons. It is worth noting that perovskites have high light absorption coefficients, long carrier diffusion lengths, low non-radiative recombination rates, high defect tolerance and easily adjustable emission wavelengths. At the same time, perovskite materials usually have exciton binding energies greater than room temperature thermal kinetic energy and high exciton concentrations. All of these make perovskite materials have good application prospects in the direction of polaritons, making them potential materials for studying the interaction between light and matter.
[0005] Although there have been studies reporting perovskite polariton lasers, these lasers were all generated under pulsed light pumping, and continuous-wave (CW) pumped perovskite lasers are the only way to electrically pumped perovskite lasers. Therefore, how to achieve continuous-wave perovskite polariton lasers is an important technical issue. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention proposes a continuous-wave perovskite polariton laser, a laser chip and a manufacturing method. By introducing a perovskite gain medium into an optical microcavity, a strong coupling relationship between excitons and photons is promoted. By further adjusting the detuning degree between the cavity mode and the polariton mode, the properties of the exciton-polaritons are regulated, so that the microcavity can generate lasers under continuous-wave pumping, thereby realizing a continuous coherent light source with an ultra-low threshold.
[0007] A continuous wave perovskite polariton laser comprises an optical microcavity, a spacer layer and a gain medium, wherein the gain medium is uniformly distributed in the microcavity.
[0008] The gain medium is a perovskite material or a mixed material containing a perovskite material, in the form of a thin film, microcrystal, phosphor, nanocrystal, quantum dot or single crystal, with a thickness of 10 nm to 1 mm.
[0009] Preferably, the composition of the perovskite material is A'2A n-1 B n X 3n+1 Or ABX3, wherein A' is an organic amine ion, A is a monovalent cation, B is a divalent metal cation, X is an anion, and n is a positive integer.
[0010] Preferably, A' is phenethylamine (PEA + ), butylamine (BA + ), ethylamine (EA + ) or a combination of one or more thereof; A cesium ion (Cs+ ), methylamine ion (MA + ), formamidinium ion (FA + ), ethylamine ion (EA + ), guanidine ion (GA + ), isopropylamine ion (IPA + ) in combination of one or more; B is lead ion (Pb 2+ ), tin ions (Sn 2+ ), Germanium ions (Ge 2+ ), indium ions (In 2+ ), bismuth ion (Bi 2+ ) in combination of one or more; X is a chloride ion (Cl - ), bromide ion (Br - ), iodide ion (I - ) or a combination of one or more thereof.
[0011] Preferably, the mixed material includes perovskite material, and one or more of organic material, quantum dot material, oxide material, III-V material, II-VI material, and rare earth material.
[0012] Preferably, the optical microcavity type is a distributed Bragg reflector (DBR), a distributed feedback Bragg grating (DFB), a photonic crystal (PC), a continuous bound state structure (BIC) or a whispering gallery mode (WGM).
[0013] The continuous wave perovskite polariton laser chip comprises the continuous wave perovskite polariton laser, an electrically driven light source and a power supply. The micro-optical cavity of the continuous wave perovskite polariton laser is fixed on the electrically driven light source. The electrically driven light source is used as a pump for the laser micro-optical cavity. The power supply is connected to the electrically driven light source to drive the electrically driven light source to emit light.
[0014] Preferably, the electrically driven light source is a combination of one or more of commercial III-V light emitting diodes (LEDs), organic light emitting diodes (OLEDs), quantum dot light emitting diodes (QD-LEDs), perovskite light emitting diodes (PeLEDs), micro light emitting diodes (micro-LEDs), laser diodes (LDs), and halogen tungsten lamps.
[0015] Preferably, the micro-optical cavity is fixed on the electrically driven light source by bonding, gluing, welding, coating or photolithography.
[0016] The preparation method of a continuous wave perovskite polariton laser specifically comprises the following steps:
[0017] Step 1: Preparation of optical microcavity
[0018] Step 2: Prepare perovskite materials and lasers
[0019] A'X, AX, BX2 and molecular additives are dissolved in a solvent to obtain a perovskite precursor solution. Perovskite materials and laser devices are prepared by a solution method, and the perovskite solution is injected into an optical microcavity and placed on a hot stage for slow heating. The perovskite single crystal is obtained by a temperature rise crystallization method to form a perovskite microcavity device.
[0020] Preferably, a multilayer dielectric layer of silicon dioxide (SiO2) / titanium dioxide (TiO2) is deposited on quartz, sapphire or flexible substrate PET by sputtering or electron beam evaporation to form a distributed Bragg reflector (DBR) with high reflectivity. The thickness of each dielectric film is λ / 4n, where λ is the central wavelength of the gain medium light emission and n is the refractive index of the dielectric layer material. A periodic array of metal pillars is deposited on a DBR reflector by thermal evaporation, and the height of the metal pillars is 10nm to 1mm. The height of the metal pillar determines the cavity length of the optical microcavity, so that the detuning degree between the cavity mode and the exciton mode can be effectively adjusted. Another DBR reflector is pressed face-to-face downward onto the DBR deposited with the metal pillar array, and a certain pressure is applied to press it to form a vertical microcavity surface emitting laser (VCSEL) structure.
[0021] Preferably, the perovskite thin film is obtained by spin coating.
[0022] Preferably, the perovskite film and the laser device are prepared by evaporation, MOCVD, ALD, inkjet printing, vapor deposition, magnetron sputtering, and solid-state reaction.
[0023] Preferably, the solvent is a mixture of any one or more of DMF, DMSO, GBL and DMA.
[0024] Preferably, the molecular additive is a mixture of one or more of polymers, small molecules and oxides.
[0025] Preferably, the polymer is polymethyl methacrylate (PMMA), polyethylene glycol (PEG), polyethylene oxide (PEO), polyvinyl pyrrolidone (PVP), the small molecule is potassium bromide (KBr), potassium thiocyanate (KSCN), guanidine thiocyanate (GASCN), and the oxide is NiOx, ZnO, SnO2.
[0026] The method for preparing a continuous wave perovskite polariton laser chip uses UV epoxy resin to form a perovskite laser chip by directly attaching a perovskite microcavity to a commercial gallium nitride (GaN) LED. The GaN LED acts as a pump for the perovskite microcavity and is driven by a power supply.
[0027] The present invention has the following beneficial effects:
[0028] 1. This method uses solution method and other low-cost methods to prepare high-quality perovskite gain media, and optimizes the quality of perovskite materials by optimizing the interface, effectively suppressing the grain boundary defects and photon scattering loss problems of perovskite films, and reducing the internal loss of laser devices.
[0029] 2. This method combines high-quality optical microcavities to promote strong coupling between excitons and photons, and prepares perovskite polaritons laser devices with extremely low thresholds, which can emit laser beams under very low-power pumping conditions. Its threshold is 1-3 orders of magnitude lower than that of traditional semiconductor lasers, and its unoptimized laser threshold can reach 1-10W / cm 2 Or below, after optimization it can reach 0.1-1W / cm 2 Or below. The unoptimized laser threshold can reach 1μJ / cm under pulsed light pumping. 2 Or below, can reach 0.1μJ / cm after optimization 2 or below.
[0030] 3. This method realizes oscillation feedback through an optical microcavity, promotes the strong interaction between excitons and photons in the perovskite material, adjusts the thickness of the gain medium, realizes the microscopic property regulation of the exciton polaritons in the optical microcavity, enhances its tendency to condense to the ground state, and forms laser emission under the continuous wave pumping mode, and its exciton lifetime can reach 1ps-100ms.
[0031] 4. The perovskite laser prepared by this method can be combined with various incoherent or coherent light sources (such as commercial III-V light-emitting diodes (LEDs), organic light-emitting diodes (OLEDs), quantum dot light-emitting diodes (QD-LEDs), perovskite light-emitting diodes (PeLEDs), micro-light-emitting diodes (micro-LEDs), laser diodes (LDs), halogen tungsten lamps, etc.) to construct electrically pumped perovskite laser chips.
[0032] 5. The laser device prepared by this method has good temporal and spatial coherence and good polarization characteristics, and can be further used in low-threshold coherent light sources, slow light devices, quantum computing, optical computing, photonic chips, optoelectronic integration and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 Characterization diagram of the continuous wave green light perovskite polariton laser device prepared in Example 1;
[0034] Figure 2 The single crystal perovskite microcavity is prepared for the continuous wave polariton laser at room temperature in Example 1;
[0035] Figure 3 The evolution process from polariton laser to photon laser in the perovskite microcavity in Example 1;
[0036] Figure 4 The effect of the detuning energy on the polariton laser in Example 1;
[0037] Figure 5 Schematic diagram of preparing a continuous wave electrically pumped perovskite laser chip in Example 2. DETAILED DESCRIPTION
[0038] The present invention will be further explained below with reference to the accompanying drawings;
[0039] Example 1
[0040] This embodiment introduces a method for preparing a continuous wave green light perovskite polariton laser device, and the specific steps are as follows:
[0041] Step 1: 10 groups of SiO2 / TiO2 dielectric layers are sputtered sequentially on a quartz substrate, with the thickness of the SiO2 layer being 91 nm and the thickness of the TiO2 layer being 55 nm, to form a DBR reflector with high reflectivity (>98%).
[0042] Step 2: Use thermal evaporation to deposit periodic gold columns on the DBR reflector through a designed mask. The diameter of the gold columns is 1 mm and the period is 1 mm.
[0043] Step 3: Spin-coat a layer of PMMA on the DBR reflector to improve the surface hydrophobicity. The concentration of PMMA solution is 5 mg / ml, the spin-coating speed is 3000 rpm, and after spin-coating, heat on a hot stage at 120°C for 10 minutes for curing.
[0044] Step 4: Glue the top DBR reflector and the bottom DBR reflector prepared in step 3 face to face and fix them with clips to form a vertical microcavity structure.
[0045] Step 5: The perovskite precursor solution is made by dissolving FABr:MABr:PbBr2 with a molar ratio of 0.1:0.9:1 in a 1 mol L -1 1 mL of a mixed solvent of DMF and DMSO, wherein the ratio of DMF to DMSO is 4:1.
[0046] Step 6: Add 5 mg of molecular additive PVP to passivate defects.
[0047] Step 7: Inject the perovskite solution into the microcavity along the edge through a pipette, and use the capillary force to make the perovskite solution diffuse evenly in the microcavity.
[0048] Step 8: Place the microcavity sample containing the perovskite solution on a hot stage, and slowly increase the temperature from 30°C to 80°C at a rate of 2°C per hour. Continue heating for 24 hours after reaching 80°C. After the hot stage temperature gradually cools to room temperature, take out the microcavity device, and the perovskite polariton laser device is ready.
[0049] Step 9: Place the device on an inverted microscope platform, focus the continuous laser with a wavelength of 405nm onto the gain medium layer of the device through a 100X lens, and place a wheel-type attenuation plate in front of the objective lens to adjust the excitation intensity.
[0050] Step 10: The light beam generated by the device passes through the microscope objective lens, then through a 4f system, and is introduced into the slit entrance of the imaging spectrometer to measure its angular resolved spectrum.
[0051] Step 11: Place a polarizer in front of the imaging spectrometer, rotate the angle of the polarizer, and measure the polarization of the generated laser beam.
[0052] Step 12: The light beam of the polariton laser device is split into two beams after passing through a beam splitter. The two light beams are respectively introduced into fiber-coupled single-photon detectors to measure the temporal and spatial coherence of the light beams.
[0053] Figure 1 Figure 1 is a diagram of the preparation and material characterization of perovskite polariton lasers. a is a schematic diagram of a continuous wave perovskite polariton laser. The perovskite single crystal is sandwiched between a pair of highly reflective DBRs, and continuous wave lasers are achieved through the interaction between excitons and photons. b is a scanning transmission electron microscope (STEM) and energy dispersive spectroscopy (EDS) image of the DBR structure, showing a double layer of SiO2 and TiO2 dielectric layers. c is a flow chart of the preparation process of a single crystal perovskite microcavity. d is a scanning electron microscope (SEM) image of a MAPbBr3 perovskite single crystal, from which it can be seen that the perovskite dielectric layer is very smooth and there are no grain boundaries inside, so the scattering loss of photons is very small. e is a fluorescence microscope image of a MAPbBr3 perovskite single crystal, from which it can be seen that the fluorescence distribution is very uniform and there are no obvious defects. f is the XRD spectrum of MAPbBr3 single crystal and polycrystalline samples, from which it can be seen that the single crystal XRD has fewer impurity peaks and a narrower peak shape, indicating that the single crystal perovskite has a higher phase purity. g is the absorption spectrum and fluorescence (PL) spectrum of MAPbBr3 perovskite single crystal. h is the transient PL decay curve of the perovskite sample (excitation wavelength: 400 nm; excitation intensity: 4.2 μJ cm -2 ), where FMPB is FA 0.1 MA 0.9The abbreviation of PbBr3 perovskite. i is the fluorescence quantum efficiency (PLQY) of different perovskite samples as a function of excitation intensity. It can be seen that through strategies such as A-site cation regulation, mixed solvents, molecular additive passivation, and surface hydrophobic regulation, the final FA 0.1 MA 0.9 The PbBr3 perovskite sample has a longer fluorescence lifetime (420ns) and higher fluorescence quantum efficiency (>30%).
[0054] Figure 2 Continuous wave polariton laser of single crystal perovskite microcavity at room temperature. Where a is the evolution of emission spectrum under different continuous wave pump intensities. The inset shows the emission near-field images with pump intensities below (left), close to (middle) and above (right) the threshold. The scale bar is 20μm. b is the variation of light output intensity and spectral half-peak width with continuous pump intensity, and the pump spot diameter is 18μm. The pump intensity reported in this work is the original intensity of the incident beam (without any correction for reflection and transmission losses). c is the spatiotemporal coherence of the continuous wave exciton laser. Above the threshold, the first-order coherence g is measured using a Michelson interferometer. 1 (τ). The red solid line represents the Gaussian fit to the data. The inset shows the Michelson interference pattern at zero delay. d is the value above the laser threshold (3.2P th ). The straight line represents the dispersion relation of the exciton. The solid parabolic curve represents the dispersion relation of the cavity photons. The dotted line represents the dispersion curve of the lower polariton branch. Above the laser threshold, polaritons condense at the bottom of the lower branch to produce polariton lasers. e is the occupancy distribution curve of polaritons in various energy states when the pump intensity is lower than 0.8Pth, about 1.0Pth and higher than 2.0Pth, plotted on a semi-logarithmic scale. For each pump intensity, the zero point of the energy scale corresponds to the spatial plane wave vector k / / = 0 ground state energy, the horizontal axis represents relative k / / = 0. We assign the ground state polariton occupied state density to 1. The blue dashed line represents the Maxwell-Boltzmann distribution function at room temperature, which is in good agreement with the polariton occupied state distribution curve at the threshold, proving Bose-Einstein condensation. f is a comparison of the continuous wave laser thresholds of lasers based on different types of semiconductor materials. It can be seen that the perovskite polariton threshold we achieved is 27 times lower than that of traditional III-V semiconductors, reaching 1-2 orders of magnitude.
[0055] Figure 3 The evolution process of polariton laser to photon laser in single crystal perovskite microcavity is shown. a is the emission intensity-pump flux curve of single crystal perovskite microcavity. When the pump flux is 0.3 μJ cm -2 and 12.4 μJ cm -2When corresponds to polariton laser and photon laser respectively. A 400nm fs laser (pulse width of 270fs, repetition frequency of 50kHz) is used to pump the microcavity sample. b is the FWHM and wavelength blue shift with the change of pump flux, showing significant changes at two thresholds. The shaded area is the area near the threshold. c is the spontaneous emission spectrum, polariton laser and photon laser spectrum of single crystal perovskite. It can be found that the spectrum of polariton laser is blue-shifted compared with photon laser. d is the polarization characteristics of spontaneous radiation, polariton laser and photon laser. It can be found that both exciton polariton laser and photon laser have obvious polarization characteristics, but the polarization degree of photon laser is stronger. e is the second-order coherence function of polariton laser and photon laser g 2 (0). The gray shaded area indicates the photon laser state. f, g, h, and i show the angle-resolved emission spectra of the single crystal perovskite microcavity at different pump flow rates, where (f) P = 0.8Pth1, (g) P = 2Pth1, (h) P ~ Pth2, and (i) P = 1.6Pth2. Pth1 and Pth2 correspond to the polariton laser and photon laser thresholds, respectively. It can be seen that the energy distribution in the polariton laser mode is at the bottom of the polariton lower branch, and the energy distribution in the photon laser mode is at the bottom of the cavity mode, which is relatively blue-shifted.
[0056] Figure 4 The effect of detuning energy on polariton lasing is demonstrated. Detuning energy refers to the energy difference (△) between the cavity mode and the exciton mode. Among them, a, b, and c are the angle-resolved emission spectra of the single crystal perovskite microcavity when △ = -50, △ = -35, and △ = -18meV, respectively. It can be found that as the detuning energy (absolute value) gradually decreases, the polaritons condense better. d is the polariton occupation function at different detuning energies. e is the emission intensity-pump flux characteristics at detuning energies △ = -78, -50, -35, and -18meV. It can be found that the threshold will decrease as the detuning energy (absolute value) gradually decreases. f is the relationship between the laser threshold and the detuning energy. For the cases of △ <-60meV and △ > 0meV (positive detuning energy), no continuous wave polariton lasing was observed.
[0057] Example 2
[0058] This embodiment introduces a method for preparing a continuous wave electrically pumped perovskite laser chip, and the specific steps are as follows:
[0059] Step 1: 10 groups of SiO2 / TiO2 dielectric layers are sputtered sequentially on a quartz substrate, with the thickness of the SiO2 layer being 91 nm and the thickness of the TiO2 layer being 55 nm, to form a DBR reflector with high reflectivity (>98%).
[0060] Step 2: Use thermal evaporation to deposit periodic gold columns on the DBR reflector through a designed mask. The diameter of the gold columns is 1 mm and the period is 1 mm.
[0061] Step 3: Spin-coat a layer of PMMA on the DBR reflector to improve the surface hydrophobicity. The concentration of PMMA solution is 5 mg / ml, the spin-coating speed is 3000 rpm, and after spin-coating, heat on a hot stage at 120°C for 10 minutes for curing.
[0062] Step 4: Glue the top DBR reflector and the bottom DBR reflector prepared after step 3 face to face and fix them with clips to form a vertical microcavity structure.
[0063] Step 5: The perovskite precursor solution is made by dissolving FABr:MABr:PbBr2 with a molar ratio of 0.1:0.9:1 in a 1 mol L -1 1 mL of a mixed solvent of DMF and DMSO, wherein the ratio of DMF to DMSO is 4:1.
[0064] Step 6: Add 5 mg of molecular additive PVP to passivate defects.
[0065] Step 7: Inject the perovskite solution into the microcavity along the edge through a pipette. Using the capillary force, the perovskite solution will diffuse evenly in the microcavity.
[0066] Step 8: Place the microcavity sample containing the perovskite solution on a hot stage, and slowly increase the temperature from 30°C to 80°C, increasing by 2°C every hour. Continue heating for 24 hours after reaching 80°C, and take out the microcavity device after the hot stage temperature gradually cools to room temperature.
[0067] Step 9: A commercial GaN LED chip was attached to the bottom of the microcavity device using epoxy.
[0068] Step 10: Use a DC current source to drive the GaN LED and collect the light beam emitted from the top of the microcavity device into a spectrometer to measure the spectrum. Place a long-pass filter (>500nm) in front of the spectrometer to filter the pump light source.
[0069] Figure 5The preparation and effect diagram of the electrically pumped laser chip, where a is a schematic diagram of the electrically injected perovskite laser chip, which is powered by a DC current source for a 450nm GaN LED. b is the emission intensity and spectral half-peak width of the perovskite polariton laser chip as the GaN LED DC drive current changes. It can be seen that the emission intensity has an obvious increase near the current threshold. At the same time, the spectral half-peak width also drops sharply from 1.8nm to 0.8nm. These features all verify the generation of lasers. c is the laser spectrum of microcavities of different lengths (adjusted by the thickness of the single crystal). Under a driving current of 60mA, the adjustable laser wavelength of 545~557nm is achieved.
[0070] Example 3
[0071] This embodiment introduces a method for preparing a continuous wave near-infrared perovskite polariton laser device, and the specific steps are as follows:
[0072] Step 1: 10 groups of SiO2 / TiO2 dielectric layers are sputtered sequentially on a quartz substrate, with the thickness of the SiO2 layer being 130 nm and the thickness of the TiO2 layer being 78 nm, to form a DBR reflector with high reflectivity (>98%) in the near-infrared region.
[0073] Step 2: Use thermal evaporation to deposit periodic gold columns on the DBR reflector through a designed mask. The diameter of the gold columns is 1 mm and the period is 1 mm.
[0074] Step 3: Spin-coat a layer of PMMA on the DBR reflector to improve the surface hydrophobicity. The concentration of PMMA solution is 5 mg / ml, the spin-coating speed is 3000 rpm, and after spin-coating, heat on a hot stage at 120°C for 10 minutes for curing.
[0075] Step 4: Glue the top DBR reflector and the bottom DBR reflector prepared after step 3 face to face and fix them with clips to form a vertical microcavity structure.
[0076] Step 5: The perovskite precursor solution is made by dissolving FABr:MABr:PbBr2 with a molar ratio of 0.1:0.9:1 in a 1 mol L -1 1 mL of a mixed solvent of DMF and DMSO, wherein the ratio of DMF to DMSO is 4:1.
[0077] Step 6: Add 5 mg of molecular additive PVP to passivate defects.
[0078] Step 7: Inject the perovskite solution into the microcavity along the edge through a pipette. Using the capillary force, the perovskite solution will diffuse evenly in the microcavity.
[0079] Step 8: Place the microcavity sample containing the perovskite solution on a hot stage, and slowly increase the temperature from 30°C to 120°C, increasing by 3°C every hour. Continue heating for 24 hours after reaching 120°C. After the hot stage temperature gradually cools to room temperature, take out the microcavity device, and the perovskite polariton laser device is ready.
[0080] Step 9: Place the device on an inverted microscope platform, focus the continuous laser with a wavelength of 532nm through a 100x lens onto the gain medium layer of the device, and place a wheel-type attenuation plate in front of the objective lens to adjust the excitation intensity.
[0081] Step 10: The light beam generated by the device passes through the microscope objective lens, then through a 4f system, and is introduced into the slit entrance of the imaging spectrometer to measure its angular resolved spectrum.
[0082] Step 11: Place a polarizer in front of the imaging spectrometer, rotate the angle of the polarizer, and measure the polarization of the generated laser beam.
[0083] Step 12: The light beam of the polariton laser device is split into two beams after passing through a beam splitter. The two light beams are respectively introduced into fiber-coupled single-photon detectors to measure the temporal and spatial coherence of the light beams.
[0084] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any researchers and technicians familiar with the field, within the technical scope described in the present invention, who make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention, should be covered by the protection scope of the present invention.
Claims
1. A continuous wave perovskite polariton laser comprising an optical microcavity, a spacer layer and a gain medium, characterized in that: The preparation method of the continuous wave perovskite polariton laser is as follows: Step 1: Preparation of optical microcavity A periodic metal column array is deposited on a DBR reflector, wherein the height of the metal column is 10 nm to 1 mm; another DBR reflector faces downward and is glued face to face with the DBR on which the metal column array is deposited, and a certain pressure is applied to press the DBR to form a vertical microcavity surface emitting laser VCSEL structure; Step 2: Preparation of perovskite materials A'X, AX, BX2 and molecular additives are dissolved in a solvent to obtain a perovskite precursor solution, and a perovskite material is prepared by a solution method, wherein A' is an organic amine ion, A is a monovalent cation, B is a divalent metal cation, and X is an anion; Step 3: Prepare perovskite laser The perovskite solution is injected into the optical microcavity and placed on a hot stage for slow heating and crystallization, so that the perovskite single crystal is grown in situ to obtain a continuous wave perovskite polariton laser. The continuous wave perovskite polariton laser operates in a continuous wave pumping mode, based on the polariton condensation emission, and the laser threshold is as low as 0.4 W cm -2 ; The gain medium is a perovskite material, which is evenly distributed in the microcavity.
2. The continuous wave perovskite polariton laser according to claim 1, characterized in that: The composition of the perovskite material is A'2A n-1 B n X 3n+1 or ABX3, n is a positive integer; A' is phenethylamine PEA + , butylamine BA + , ethylamine EA + A cesium ion Cs + , methylamine ion MA + , formamidinium ion FA + , ethylamine ion EA + , guanidine ion GA + 、Isopropylamine ion IPA + One or more combinations thereof; B is lead ion Pb 2+ 、Sn 2+ 、Ge 2+ 、Indium ion In 2+ 、Bi ion 2+ One or more combinations of; X is a chloride ion Cl - 、Br - 、Iodide ion I - A combination of one or more of .
3. The continuous wave perovskite polariton laser according to claim 1, characterized in that: On quartz, sapphire or flexible substrate PET, a multi-layer dielectric layer of silicon dioxide SiO2 / titanium dioxide TiO2 is deposited by sputtering or electron beam evaporation to form a distributed Bragg reflector DBR with high reflectivity; the thickness of each dielectric film is λ / 4n, where λ is the central wavelength of the gain medium light emission and n is the refractive index of the dielectric layer material.
4. The continuous wave perovskite polariton laser according to claim 1, characterized in that: The solvent is any one or more mixtures of DMF, DMSO, GBL, and DMA; the molecular additive is any one or more mixtures of polymers, small molecules, and oxides.
5. The continuous wave perovskite polariton laser according to claim 4, characterized in that: The polymers are polymethyl methacrylate PMMA, polyethylene glycol PEG, polyethylene oxide PEO, polyvinyl pyrrolidone PVP, the small molecules are potassium bromide KBr, potassium thiocyanate KSCN, guanidine thiocyanate GASCN, and the oxides are NiOx, ZnO, and SnO2.
6. A continuous wave perovskite polariton laser chip, comprising a laser, an electrically driven light source and a power supply, characterized in that: The laser is a continuous wave perovskite polariton laser as described in any one of claims 1 to 5; the micro-optical cavity of the continuous wave perovskite polariton laser is fixed on an electrically driven light source; the electrically driven light source serves as a pump for the laser micro-optical cavity; the power supply is connected to the electrically driven light source to drive the electrically driven light source to emit light.
7. The continuous wave perovskite polariton laser chip according to claim 6, characterized in that: The micro-optical cavity is fixed on the electrically driven light source by bonding, gluing, welding, coating or photolithography, and the electrically driven light source serves as a pump for the micro-optical cavity.