Application of polycrystalline diamond composite sheet in the swash plate and / or valve plate of plunger pump

By using polycrystalline diamond composite sheets to improve the friction and wear characteristics and sealing performance of the plunger pump swash plate and dispensing plate, the wear and leakage problems of traditional materials at high speeds and high pressures are solved, and ultra-high pressure liquid transportation and long life are achieved effect.

CN117738862BActive Publication Date: 2024-11-26BEIJING NINGHUA DIAMOND BEARING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410037539.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-10
Publication Date
2024-11-26
Estimated Expiration
2044-01-10

AI Technical Summary

Technical Problem

Friction pair wear in the plunger pump leads to leakage, reduced efficiency and system heating, especially under high speed and high pressure conditions, traditional materials are difficult to meet the requirements of ultra-high pressure liquid delivery.

Method used

The polycrystalline diamond composite sheet is used as the material of the plunger pump swash plate and the distribution plate, and is prepared by mixing and sintering of diamond and catalyst to form a composite sheet with high thermal conductivity, wear resistance and impact resistance, which is used to improve friction and wear characteristics. and sealing performance.

Benefits of technology

It significantly improves the working speed of the plunger pump, extends its life, enhances high temperature and corrosion resistance, and is suitable for liquid transportation under high pressure, high temperature and harsh working conditions, avoiding high heat damage during start and stop .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117738862B_ABST
    Figure CN117738862B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of hydraulic pump accessories, and specifically relates to the application of polycrystalline diamond composite sheets in the swash plate and / or the distributor plate of a plunger pump, wherein the polycrystalline diamond composite sheet comprises: a substrate having an upper surface; and a polycrystalline diamond layer arranged on the upper surface of the substrate. The preparation method of the polycrystalline diamond composite sheet comprises the following steps: mixing diamond powder with a catalyst to obtain a diamond mixture; then assembling the diamond mixture with a substrate to obtain a blank; and sintering the blank at high temperature and high pressure to obtain a polycrystalline diamond composite sheet. The swash plate and / or distributor plate manufactured by the present invention using the polycrystalline diamond composite sheet have the characteristics of high wear resistance, high thermal conductivity, friction coefficient, extremely low thermal expansion coefficient, etc., and are suitable for harsh working conditions requiring high speed, high pressure, large displacement, high liquid temperature, corrosive liquid, and liquid containing a large number of highly abrasive solid phase particles, and are also suitable for dry grinding conditions at low speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydraulic pump accessories, and in particular relates to the application of a polycrystalline diamond composite sheet in a swash plate and / or a port plate of a plunger pump. Background Art

[0002] The plunger pump is an important device in the hydraulic system. The lubrication and wear of the three key friction pairs in the plunger pump, namely the slipper pair, the plunger pair and the flow distribution pair, are the decisive factors for the performance and service life of the plunger pump. Wear of the friction pair of the plunger pump will lead to the expansion of the gap between the friction surfaces, increase the leakage inside the plunger pump, reduce the volumetric efficiency of the components, increase the heating of the system, and eventually lead to damage to the plunger pump. The wear and failure of the key friction pair is an important factor affecting the life and pressure of the plunger pump. Among them, the slipper pair is the contact surface between the slipper and the swash plate. At the low-speed stage when the oil film has not yet formed, or at the ultra-high-speed operation stage, the swash plate is very easy to wear; among them, the flow distribution pair is the largest friction pair in the single structure of the plunger pump, and while satisfying the flow distribution function, it also plays the role of supporting the cylinder body to maintain the force balance of the cylinder body. Therefore, the flow distribution pair is also the most prone to wear and even burning the plate. Summary of the invention

[0003] In view of the deficiencies in the prior art, the present invention provides the use of a polycrystalline diamond composite sheet in a swash plate and / or a distributor plate of a plunger pump.

[0004] Specifically, the present invention provides the following technical solutions:

[0005] A polycrystalline diamond composite sheet is used in manufacturing a swash plate and / or a valve plate of a plunger pump, wherein the polycrystalline diamond composite sheet comprises:

[0006] a substrate having an upper surface;

[0007] The polycrystalline diamond layer is arranged on the upper surface of the substrate.

[0008] The inventor of the present invention unexpectedly discovered that the plunger pump swash plate and / or distribution plate made by using polycrystalline diamond composite sheets as raw materials can not only double the maximum operating speed, but also greatly improve the friction and wear characteristics, lubrication characteristics and sealing performance of the sliding shoe pair and / or distribution pair, and are suitable for harsh working conditions such as high speed, high pressure, large displacement, wear resistance, long life, stable operation, high liquid temperature, corrosive liquid, unclean liquid containing a large number of highly abrasive solid particles. In particular, when the oil film has not yet been formed at a low speed, the plunger pump swash plate does not need lubrication. Due to its extremely low friction coefficient and high thermal conductivity, it can avoid damage to the material caused by the high heat generated during the start or stop of the plunger pump. This solves the bottleneck problem that restricts the long-term stable operation of the plunger pump.

[0009] Preferably, the thickness of the polycrystalline diamond layer is 0.01 mm to 3 mm, and more preferably 0.5 mm to 2 mm. If the thickness is too small, it may not be able to effectively realize its function, and if the thickness is too large, the internal structure is uneven, which has the disadvantages of increased cost and excessive processing time.

[0010] Preferably, the material of the substrate is cemented carbide, more preferably at least one of WC-Co cemented carbide, tungsten-titanium-cobalt cemented carbide, tungsten-titanium-tantalum cemented carbide, and tungsten-titanium-niobium cemented carbide; more preferably WC-Co cemented carbide.

[0011] Preferably, the thickness of the substrate is less than 8 mm; more preferably 2-5 mm.

[0012] Preferably, the method for preparing the polycrystalline diamond compact comprises the following steps:

[0013] 1) mixing diamond powder with a catalyst to obtain a diamond mixture; then assembling the diamond mixture with the substrate to obtain a blank; the catalyst contains Co;

[0014] 2) Sintering the blank to obtain the polycrystalline diamond composite sheet.

[0015] Preferably, the catalyst is a mixture of Co, Fe and Ni. The present invention finds that by adding the above-mentioned specific catalyst to diamond powder, under thermodynamic conditions, diamond carbon atoms dissolve in the catalyst liquid and are deposited on the surface of diamond particles in atomic form to form a DD bond structure. One of the key technologies in production is to achieve uniform diffusion and penetration of metal catalysts and control the kinetic conditions for achieving diamond recrystallization.

[0016] Further preferably, based on the mass of the diamond powder, the amount of Co in the catalyst is 5%-15%, the amount of Fe is 4‰-6‰, and the amount of Ni is 2‰-4‰. Experiments have found that the mechanical properties of the prepared plunger pump swash plate and / or valve plate are significantly different when the amount ratio of Co, Fe, and Ni is different. Within the above amount range, the synergistic effect of Co, Fe, and Ni can greatly improve the toughness and impact resistance of the material, so that it is not easy to collapse and crack during use, especially in a high-speed working environment.

[0017] Most preferably, based on the mass of the diamond powder, the amount of Co in the catalyst is 9%-11%, the amount of Fe is 4‰-6‰, and the amount of Ni is 2‰-4‰. Under the above dosage ratio, the obtained inclined plate and / or distribution plate has the best toughness and impact resistance.

[0018] Preferably, the diamond powder is first subjected to vacuum purification treatment and then mixed with the catalyst. The present invention requires that the diamond powder is first subjected to vacuum purification treatment to remove suspended gas adsorbed on the surface of the diamond powder.

[0019] Preferably, the particle size of the diamond powder is 0.2 μm-40 μm; more preferably 10 μm-35 μm;

[0020] And / or, the particle size of the catalyst is 0.2 μm-40 μm; more preferably 10 μm-35 μm;

[0021] And / or, the particle size of the diamond powder is the same as the particle size of the catalyst.

[0022] Within the above particle size range, the catalyst has the best dispersibility in diamond powder.

[0023] Preferably, the sintering is specifically as follows: the blank is first pressurized to 5.0-8.0 Gpa, then heated to 1450-1600° C., and kept at this temperature for 5-30 minutes. After the sintering is completed, the blank is depressurized, cooled, and the sintered polycrystalline diamond composite is taken out.

[0024] It is well known in the art that polycrystalline diamond composite sheets are highly sensitive to sintering process conditions. The present invention finds that the polycrystalline diamond composite sheets sintered within the above-mentioned pressure, temperature and time range have various properties that are more suitable for the operating conditions of the swash plate and / or the distributor plate of the plunger pump.

[0025] Preferably, at least one of laser processing, mechanical processing and electrical discharge processing is used to process the polycrystalline diamond composite sheet into the desired shape of the inclined plate and / or the distribution plate through the steps of drilling, grinding and polishing, cutting and forming.

[0026] Preferably, the plunger pump swash plate and / or distribution plate are used to transport ultra-high pressure liquids. It is well known in the art that an increase in rotation speed will lead to an increase in friction, an increase in temperature, and at the same time, the problem of cavitation becomes serious. The swash plate and / or distribution plate manufactured by the present invention using polycrystalline diamond composite sheets have excellent wear resistance, thermal conductivity, toughness and impact resistance, can operate under high temperature conditions, avoid thermal melting, and have excellent anti-cavitation effects, and are suitable for high operating speeds, thereby enabling ultra-high pressure liquid transportation. However, the existing swash plates and / or distribution plates made of integral brass, 38CrMoAl, 42CrMo and other low-alloy steels, and steel / copper bimetallics generally wear rapidly under high-speed conditions due to the large friction coefficient, relatively poor wear resistance, large thermal expansion coefficient, etc., resulting in the inability to achieve ultra-high pressure liquid transportation.

[0027] The pressure of ultra-high pressure liquid delivery is usually higher than that of ordinary liquid delivery systems. The specific pressure requirements of ultra-high pressure liquid delivery will vary according to the requirements of the application and system design, but generally, the pressure of ultra-high pressure liquid delivery can be above 1000 bar (equivalent to 100 MPa, or about 14500 psi). This high pressure is usually used for some special applications, such as:

[0028] Chemical industry: used for transporting reactants in high-pressure reactors;

[0029] Oil and gas extraction: used to extract crude oil or natural gas from deep wells;

[0030] Material processing: for high-pressure water jet cutting, forming and cleaning;

[0031] High-pressure water treatment: used for water jet cutting, cleaning and removal of surface coatings;

[0032] Laboratory Applications: In scientific research, used in material science, geology and chemistry experiments.

[0033] Preferably, the plunger pump swash plate and / or distributor plate are used to transport low-viscosity liquids; more preferably, the low-viscosity liquid is water or aviation kerosene. The lower the viscosity of the liquid, the greater the friction resistance, and the greater the loss to the swash plate and / or distributor plate. The swash plate and / or distributor plate made of polycrystalline diamond composite sheets in the present invention are particularly suitable for transporting low-viscosity liquids and have a long working life.

[0034] Preferably, the plunger pump swash plate and / or distribution plate is used to transport liquid containing highly abrasive solid particles.

[0035] The beneficial effects of the present invention are at least:

[0036] The swash plate and / or distribution plate manufactured by the present invention using polycrystalline diamond composite sheets have excellent wear resistance and impact resistance, and the working speed is doubled. It is particularly suitable for plunger pumps that require high pressure and large displacement, and can greatly extend the life of the swash plate and / or distribution plate of the plunger pump, which is several times or even dozens of times the life of traditional materials; it can resist vaporization and increase the stability of the rotary plunger pump; at the same time, it has excellent thermal conductivity, high temperature resistance, and corrosion resistance, and is suitable for use under harsh working conditions such as high temperature, containing corrosive chemicals, and containing a large amount of highly abrasive solid particles, and can avoid damage to the bearing material caused by the high heat generated during the start or stop of the wear-resistant parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. It is obvious that the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 This is a schematic diagram of a polycrystalline diamond composite sheet prepared in Example 1; wherein, 1-polycrystalline diamond, 2-hard alloy.

[0039] Figure 2 Schematic diagram of the plunger pump swash plate prepared in Example 1.

[0040] Figure 3 The schematic diagram of the piston pump distribution plate prepared in Example 7. Among them, 1-axial piston pump oil distribution plate body, 2-unloading groove, 3-damping hole, 4-waist-shaped distribution window hole, 5-pin hole. DETAILED DESCRIPTION

[0041] The present invention is described below by the best embodiment. It should be known to those skilled in the art that the embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product manual shall be followed.

[0043] Example 1

[0044] This embodiment provides a plunger pump swash plate, the material of which is a polycrystalline diamond composite sheet, and the polycrystalline diamond composite sheet includes:

[0045] A WC-Co type cemented carbide substrate with a thickness of 5 mm, having an upper surface;

[0046] A polycrystalline diamond layer with a thickness of 1 mm is arranged on the upper surface of the substrate.

[0047] The method for preparing the above plunger pump swash plate comprises the following steps:

[0048] 1) Processing a WC-Co cemented carbide substrate into a cylindrical shape with a thickness of less than 10 mm, weighing a raw material diamond powder of about 25 μm, placing it in a vacuum purification device, and performing vacuum purification treatment to remove suspended gas adsorbed on the surface of the diamond powder, adding a catalyst of about 25 μm (the catalyst is a mixture of 10% Co, 5‰ Fe, and 3‰ Ni) to the purified raw material diamond powder, and mixing them evenly to obtain a diamond mixture, then loading the processed cemented carbide substrate into a metal molybdenum cup, loading the diamond mixture into one end face of the cemented carbide substrate, and then assembling it in a pyrophyllite cavity, and then placing the assembled pyrophyllite cavity on a six-sided top ultra-high pressure and high temperature device, using a sintering process of first increasing the pressure to 6.5 Gpa and then increasing the temperature, when the temperature rises to 1450-1500°C, sintering for 15 minutes, stopping the heat and depressurizing and cooling, to obtain a sintered polycrystalline diamond composite sheet, Figure 1 Schematic diagram of the polycrystalline diamond composite sheet prepared in Example 1.

[0049] 2) The polycrystalline diamond composite sheet is processed into a Figure 2 The shape of the inclined disk; the flatness of the surface of the polycrystalline diamond layer is less than 0.005mm.

[0050] Example 2

[0051] The only difference between Example 2 and Example 1 is that the catalyst is a mixture of 10% Co, 5‰ Fe, and 1‰ Ni.

[0052] Example 3

[0053] The only difference between Example 3 and Example 1 is that the catalyst is a mixture of 10% Co, 5‰ Fe, and 5‰ Ni.

[0054] Example 4

[0055] The only difference between Example 4 and Example 1 is that the catalyst is a mixture of 10% Co, 3‰ Fe, and 3‰ Ni.

[0056] Example 5

[0057] The only difference between Example 5 and Example 1 is that the catalyst is a mixture of 10% Co, 8‰ Fe, and 3‰ Ni.

[0058] Example 6

[0059] The only difference between Example 6 and Example 1 is that the catalyst contains 10% Co.

[0060] Comparative Example 1

[0061] Comparative Example 1 provides a conventional plunger pump swash plate, which is different from Example 1 only in that the plunger pump swash plate is made of 38CrMoAl and has a thickness of 2.8 mm.

[0062] The test example uses a plunger pump of model GL32 of Glencore for testing, wherein the swash plates used are the swash plates described in Examples 1-6 and Comparative Example 1, respectively.

[0063] 1. Test the PV limit value that the swash plate in the plunger pump can withstand (the increase in operating speed will inevitably increase the PV value that the swash plate can withstand). In the mechanical seal manufacturing industry, the PV value is used to indicate the working capacity of the mechanical seal. The higher the PV value of the mechanical seal, the stronger the working capacity of the mechanical seal. Among them, P-seal fluid pressure (Mpa); V-average sliding speed of the seal end face (m / s).

[0064] 2. Use the plunger pump to deliver conventional hydraulic oil and test the maximum operating speed that the swash plate can withstand.

[0065] 3. Operate the plunger pump at 6000 rpm to transport low-viscosity medium aviation kerosene and test the service life of the swash plate.

[0066] The performance data are summarized in Table 1, where the *data are normalized relative to Comparative Example 1.

[0067] Table 1

[0068]

[0069] Example 7

[0070] This embodiment provides a plunger pump valve plate, the material of which is a polycrystalline diamond composite sheet, and the polycrystalline diamond composite sheet includes:

[0071] A WC-Co type cemented carbide substrate with a thickness of 5 mm, having an upper surface;

[0072] A polycrystalline diamond layer with a thickness of 1 mm is arranged on the upper surface of the substrate.

[0073] The method for preparing the plunger pump valve plate comprises the following steps:

[0074] 1) The preparation method of the polycrystalline diamond composite sheet is the same as that of Example 1;

[0075] 2) The polycrystalline diamond composite sheet is processed into a Figure 3 The shape of the distribution plate; the flatness of the surface of the polycrystalline diamond layer is less than 0.005mm.

[0076] like Figure 3As shown, the polycrystalline diamond layer surface of the axial piston pump oil distribution plate body (1) is provided with four unloading grooves (2) and four mutually symmetrical damping holes (3), and the oil distribution plate body (1) is provided with four waist-shaped distribution window holes (4) and one pin hole (5).

[0077] Example 8

[0078] The only difference between Example 8 and Example 7 is that the catalyst is a mixture of 10% Co, 5‰ Fe, and 1‰ Ni.

[0079] Example 9

[0080] The only difference between Example 9 and Example 7 is that the catalyst is a mixture of 10% Co, 5‰ Fe, and 5‰ Ni.

[0081] Example 10

[0082] The only difference between Example 10 and Example 7 is that the catalyst is a mixture of 10% Co, 3‰ Fe, and 3‰ Ni.

[0083] Embodiment 11

[0084] The only difference between Example 11 and Example 7 is that the catalyst is a mixture of 10% Co, 8‰ Fe, and 3‰ Ni.

[0085] Example 12

[0086] The only difference between Example 12 and Example 7 is that the catalyst contains 10% Co.

[0087] Comparative Example 2

[0088] Comparative Example 2 provides a traditional plunger pump valve plate, which is different from Example 7 only in that the plunger pump valve plate is made of 38CrMoAl and has a thickness of 2.8 mm.

[0089] Test example

[0090] The test was conducted using a Glan Zhongchuang GL32 plunger pump, wherein the distribution plates used were the distribution plates described in Examples 7 to 12 and Comparative Example 2, respectively.

[0091] 1. Test the PV limit value that the valve plate in the plunger pump can withstand (the increase in operating speed will inevitably increase the PV value that the inclined plate can withstand). In the mechanical seal manufacturing industry, the PV value is used to indicate the working capacity of the mechanical seal. The higher the PV value of the mechanical seal, the stronger the working capacity of the mechanical seal. Among them, P-seal fluid pressure (Mpa); V-average sliding speed of the seal end face (m / s).

[0092] 2. Use the plunger pump to deliver conventional hydraulic oil and test the maximum operating speed that the valve plate can withstand.

[0093] 3. Operate the plunger pump at 6000 rpm to transport low-viscosity medium aviation kerosene and test the service life of the distribution plate.

[0094] The performance data are summarized in Table 2, where the *data are normalized relative to Comparative Example 2.

[0095] Table 2

[0096]

[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. Application of polycrystalline diamond composite sheet in manufacturing swash plate and / or distributor plate of plunger pump, characterized in that: The polycrystalline diamond composite sheet comprises: a substrate having an upper surface; A polycrystalline diamond layer is disposed on the upper surface of the substrate; The method for preparing the polycrystalline diamond compact comprises the following steps: 1) mixing diamond powder with a catalyst to obtain a diamond mixture; then assembling the diamond mixture with the substrate to obtain a blank; the catalyst contains Co; 2) Sintering the blank to obtain the polycrystalline diamond composite sheet; The catalyst is a mixture of Co, Fe and Ni. Based on the mass of the diamond powder, the amount of Co in the catalyst is 9%-11%, the amount of Fe is 4‰-6‰, and the amount of Ni is 2‰-4‰.

2. The use of the polycrystalline diamond compact according to claim 1 in manufacturing a swash plate and / or a valve plate of a plunger pump, characterized in that: The thickness of the polycrystalline diamond layer is 0.01 mm-3 mm.

3. The use of the polycrystalline diamond compact according to claim 1 in manufacturing a swash plate and / or a valve plate of a plunger pump, characterized in that: The diamond powder is first subjected to vacuum purification treatment and then mixed with the catalyst.

4. The use of the polycrystalline diamond compact according to claim 1 in manufacturing a swash plate and / or a valve plate of a plunger pump, characterized in that: The particle size of the diamond powder is 0.2 μm-40 μm; And / or, the particle size of the catalyst is 0.2 μm-40 μm; And / or, the particle size of the diamond powder is the same as the particle size of the catalyst.

5. The use of the polycrystalline diamond compact according to claim 1 in manufacturing a swash plate and / or a valve plate of a plunger pump, characterized in that: The sintering is specifically as follows: the blank is firstly pressurized to 5.0-8.0 Gpa, then heated to 1450-1600°C, and kept at this temperature and pressure for 5-30 minutes.

6. Use of the polycrystalline diamond compact according to claim 1 or 2 in manufacturing a swash plate and / or a port plate of a plunger pump, characterized in that: The polycrystalline diamond composite sheet is processed into the required inclined plate and / or distributor plate shape by using at least one processing method selected from laser processing, mechanical processing and electric spark processing, and sequentially undergoing the processes of drilling, grinding, cutting and forming.

7. Use of the polycrystalline diamond compact according to claim 1 or 2 in manufacturing a swash plate and / or a port plate of a plunger pump, characterized in that: The plunger pump swash plate and / or port plate are used to transport ultra-high pressure liquid.

8. Use of the polycrystalline diamond compact according to claim 1 or 2 in manufacturing a swash plate and / or a port plate of a plunger pump, characterized in that: The plunger pump swash plate and / or distributor plate is used for conveying low-viscosity liquid or liquid containing highly abrasive solid particles.