A high-toughness gray zirconia ceramic and preparation method thereof

By using additives such as cobalt metal salt and silicon carbide fiber in yttria stable zirconia ceramics, combined with a reducing atmosphere, the problem of unstable color formation in gray zirconia ceramics during sintering is solved, and high toughness and stable gray color rendering is achieved. , suitable for high-end applications.

CN117776753BActive Publication Date: 2024-11-05JIAOZUO JINXIN HENGTUO REFRACTORIES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311831506.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-11-05
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

The existing gray zirconia ceramics are difficult to stabilize color during the sintering process, and their performance is poor, which limits their application, mainly because the extreme use temperature of tin antimony gray materials and nickel oxide, manganese oxide and other color materials is lower than the ceramic sintering temperature. Causes unstable color.

Method used

Using yttrium oxide-stabilized zirconia ceramic powder as the main material, combined with water-soluble cobalt metal salt as the colorant, through the color development reaction of cobalt ions, and using dispersants, lubricants, plasticizers and composites during the sintering process Additives such as silicon carbide fibers, combined with the reducing atmosphere, achieve stable gray color development and high toughness.

Benefits of technology

It realizes the gray color development of zirconia ceramics with stable color at room temperature, which improves the density, hardness and toughness of the ceramics, reduces color aberration, and reduces sintering temperature, and is suitable for high-end applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005041896850000151
    Figure GDA0005041896850000151
  • Figure GDA0005041896850000161
    Figure GDA0005041896850000161
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic materials, in particular to a high-toughness grey zirconia ceramic and a preparation method thereof, comprising a zirconia ceramic main material and an additive; the zirconia ceramic main material is yttria-stabilized zirconia ceramic powder; the additive comprises a colorant, a dispersant, a lubricant, a plasticizer and a composite auxiliary agent; the preparation method comprises the steps of ball milling to obtain a first slurry, adding a colorant to form a color paste, adding a composite auxiliary agent, a plasticizer and a lubricant to form a second slurry, and then subjecting the second slurry to pressure spray drying, dry pressing, debinding treatment and sintering treatment to obtain the high-toughness grey zirconia ceramic; the high-toughness grey zirconia ceramic prepared by the invention has excellent performance, can stably present a grey color after the zirconia ceramic is sintered, and can maintain high toughness under the condition of maintaining a high density, and is in line with and applicable to more high-end applications of grey zirconia ceramics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of ceramic materials technology, and in particular to a high-toughness gray zirconia ceramic and its preparation method. Background Technology

[0002] Zirconia ceramics are strong, wear-resistant, and flexible industrial ceramics. Due to their high strength, high fracture toughness, and high thermal expansion, they have wide applications in industry and daily life. Examples include automotive engine parts, brakes, piston rings, etc., in the automotive industry; mobile phones and other 3C electronics industries; and artificial joints, dental restorations, etc., in the medical industry.

[0003] In recent years, colored ceramic products, due to their unique colors and the superior properties of ceramics, have found wide application in high-end decorative fields such as ceramic covers, mobile phone back panels, mobile phone casings, watch cases, watch chains, and buttons. Among them, gray ceramic materials are widely favored by consumers for their understated, simple, high-end, and fashionable appearance. However, existing gray zirconia ceramics generally use tin-antimony gray pigments and nickel oxide and manganese oxide as gray pigments. Rutile antimony-tin gray pigments are mainly synthesized using a high-temperature solid-state synthesis method. The sintering process of this pigment requires strict atmospheric conditions, and its stable color development temperature is between 1200-1350℃, failing to exhibit good coloring effects at room temperature. Gray pigments made from oxides such as manganese oxide and nickel oxide have a maximum operating temperature below 1300℃, while the sintering temperature of zirconia ceramics is generally between 1400-1550℃. At this sintering temperature, the pigment cannot stably develop color after being fired with the ceramic, affecting the color and performance of the prepared gray ceramics. This makes current gray zirconia ceramics difficult to process, difficult to achieve stable color development, and has poor performance, thus limiting their application. Summary of the Invention

[0004] To address the above problems, this invention provides a high-toughness zirconia ceramic and its preparation method.

[0005] Firstly, one of the objectives of this invention is to provide a high-toughness gray zirconia ceramic, the technical solution of which is as follows:

[0006] A high-toughness gray zirconia ceramic includes a zirconia ceramic base material and additives; the zirconia ceramic base material is yttrium oxide stabilized zirconia ceramic powder; the additives include colorants, dispersants, lubricants, plasticizers, and composite auxiliaries.

[0007] The colorant is a cobalt metal salt that is easily soluble in water, and the amount of the colorant is 1.5-2.5% of the amount of the zirconium oxide ceramic main material.

[0008] The amount of the dispersant is 1-3% of the amount of the zirconia ceramic main material;

[0009] The amount of the lubricant used is 0.5-1.5% of the amount of the zirconia ceramic main material used;

[0010] The amount of plasticizer used is 1.0-5.5% of the amount of the zirconia ceramic main material used;

[0011] The amount of the composite additive is 0.25-1.25% of the amount of the zirconia ceramic main material.

[0012] In one embodiment, the composite additive is silicon carbide fiber.

[0013] In one embodiment, the aspect ratio of the silicon carbide fiber ranges from 15:1 to 20:1.

[0014] In one embodiment, the yttrium oxide content in the yttrium-stabilized zirconia ceramic powder is 2.5-4% of the amount of the zirconia ceramic main material.

[0015] In one embodiment, the colorant includes cobalt chloride hexahydrate and cobalt chloride.

[0016] In one embodiment, the dispersant is one or more of ammonium polyacrylate, polyethylene glycol, ammonium polymethacrylate, and sodium tripolyphosphate; the lubricant is talc or polyvinyl alcohol; and the plasticizer is one or more of hydroxymethyl cellulose, polyvinyl alcohol, and bone glue.

[0017] Secondly, the second objective of this invention is to provide a method for preparing high-toughness zirconia ceramic, the technical features of which are as follows:

[0018] A method for preparing high-toughness gray zirconia ceramic includes the following preparation steps:

[0019] S1: The zirconia ceramic host material, dispersant and pure water are mixed to form a mixed slurry, and the mixed slurry is ball-milled until a first slurry with D50 of 0.05μm to 0.25μm is formed, wherein the mass of the zirconia ceramic host material accounts for 35-50% of the mass of the mixed slurry;

[0020] S2: Add colorant to the first slurry, continue ball milling until the particle size inside the slurry tends to be uniform, then stop ball milling, adjust the slurry to be alkaline, stir evenly, and obtain color paste;

[0021] S3: Add composite additives to the color paste and disperse it fully using ultrasound. After standing for more than 24 hours, add plasticizer and lubricant and stir until it is evenly mixed to make the second paste.

[0022] S4: The second slurry is subjected to pressure spray drying, dry pressing, debinding and sintering to obtain high-toughness gray zirconia ceramic; wherein the sintering temperature is 1250-1550℃, the sintering time is 1-4h, and the sintering atmosphere is a reducing atmosphere.

[0023] In one embodiment, in step S2, the pH value of the slurry is 9-12.

[0024] In one embodiment, in step S3, the composite additive needs to be pretreated. The pretreatment step includes dispersing the composite additive in a 2-8 mol / L nitric acid solution, controlling the temperature between 40-60°C, soaking for 8-16 hours, rinsing with clean water and drying.

[0025] In one embodiment, in step S4, the reducing atmosphere is a high-purity hydrogen atmosphere, and during the sintering process, the hydrogen flow rate is controlled to be 0.5-1 L / min.

[0026] Beneficial effects: The gray zirconia ceramic of the present invention is mainly achieved through the color reaction of cobalt. Cobalt metal salt is added to the first slurry, which exists in the form of cobalt ions. At this time, the slurry is light pink. After adjusting the slurry to be alkaline, the color slurry as a whole turns blue or cyan. It is speculated that the cobalt ions exist in the form of cobalt hydroxide precipitate. Finally, during the sintering process, under the action of a reducing atmosphere, and with the synergistic effect of additives such as dispersants, lubricants, plasticizers and composite additives, the zirconia ceramic after sintering exhibits a stable gray color and has high toughness and other physicochemical properties.

[0027] Specifically, the color development principle of gray zirconia ceramics is as follows:

[0028] CoCl₂ + NaOH = Co(OH)Cl + NaCl

[0029] Co(OH)Cl+NaOH=Co(OH)2↓+NaCl

[0030] Ultimately, under the action of a reducing atmosphere, Co(OH)2 is reduced to Co metal, which makes the zirconia ceramic material stably gray.

[0031] This invention uses silicon carbide fiber as a composite additive added to color paste. Silicon carbide fiber possesses advantages such as high hardness, high strength, and high thermal stability. After being uniformly mixed with the color paste and under the action of an alkaline solution, it helps to enhance the properties of zirconia ceramics. Performance testing of the sintered zirconia ceramics showed that the addition of a specific proportion of silicon carbide fiber enhanced the toughness and hardness of the sintered zirconia ceramics to varying degrees. Color characterization of the zirconia ceramic material showed excellent stability in gray color development, without any color spots or patches. Furthermore, the pre-treated silicon carbide fiber... In addition to the aforementioned effects, the pretreated silicon carbide fibers also lower the sintering temperature of the ceramic material, thereby shortening the sintering time. They also improve properties such as density, strength, and wear resistance. Furthermore, the gray ceramic has a more stable color with less color difference between different ceramic pieces. This is presumably because a small amount of silicon carbide fibers react with alkali to generate sodium silicate or silicate derivatives, which aids in sintering. At the same time, there is a different interaction between the reacted and unreacted silicon carbide fibers compared to individual silicon carbide fibers, resulting in a stable gray color and high toughness.

[0032] The high-toughness gray zirconia ceramic prepared by this invention exhibits excellent properties. After sintering, it stably displays a gray color and maintains high toughness while preserving high density, making it suitable for a wider range of high-end applications of gray zirconia ceramics. The density of the high-toughness zirconia ceramic prepared by this invention is 6.28 g / cm³. 3 The Vickers hardness is 1250 kgf / mm². 2 The above values ​​are: three-point bending strength greater than 1300 MPa, fracture toughness greater than 12 MPa / m, and lab value range 25≤L≤40, -1≤a≤0, -2≤b≤1. Detailed Implementation

[0033] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0034] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0036] Firstly, one of the objectives of this invention is to provide a high-toughness gray zirconia ceramic that can be co-fired with zirconia ceramic and exhibits a stable gray color, and can also stably develop color when cooled to room temperature. The technical solution is as follows:

[0037] In some embodiments, the high-toughness gray zirconia ceramic includes a zirconia ceramic base material and additives; the zirconia ceramic base material is yttrium oxide stabilized zirconia ceramic powder; the additives include colorants, dispersants, lubricants, plasticizers, and composite additives.

[0038] The colorant is a water-soluble cobalt metal salt, and the amount of the colorant is 1.5-2.5% of the amount of the zirconia ceramic main material. In some specific examples, the amount of the colorant can be 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, or 2.5% of the amount of the zirconia ceramic main material.

[0039] The amount of the dispersant is 1-3% of the amount of the zirconia ceramic main material. In some specific examples, the amount of the dispersant is 1%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.5%, 2.6%, 2.8%, or 3.0% of the amount of the zirconia ceramic main material.

[0040] The amount of lubricant used is 0.5-1.5% of the amount of the zirconia ceramic main material. In some specific examples, the amount of lubricant used is 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, or 1.5% of the amount of the zirconia ceramic main material.

[0041] The amount of plasticizer used is 1.0-5.5% of the amount of the zirconia ceramic main material. In some specific examples, the amount of plasticizer used is 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5%, 5.0%, and 5.5% of the amount of the zirconia ceramic main material.

[0042] The amount of the composite additive is 0.25-1.25% of the amount of the zirconia ceramic main material. In some specific examples, the amount of the composite additive is 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%, 0.55%, 0.60%, 0.65%, 0.70%, 0.75%, 0.80%, 0.85%, 0.90%, 0.95%, 1.00%, 1.05%, 1.10%, 1.15%, 1.20%, or 1.25% of the amount of the zirconia ceramic main material.

[0043] This invention uses cobalt metal salts as gray colorants for zirconia ceramics, achieving color development through the color reaction of cobalt ions in different chemical states or forms. Cobalt can be co-fired with zirconia, and after sintering, it can stably develop color at room temperature. With the combined use of other additives, especially the synergistic effect of composite additives, the zirconia ceramics exhibit stable color development without color spots or patches, and show high toughness while increasing density.

[0044] Optionally, the composite additive is silicon carbide fiber.

[0045] By combining silicon carbide fibers with other components of this invention in a synergistic manner, the invention achieves toughening, color stabilization, and sintering assistance, resulting in gray zirconia ceramics with excellent properties.

[0046] Optionally, the aspect ratio of the silicon carbide fiber is in the range of 15:1-20:1. In some specific examples, the aspect ratio of the silicon carbide fiber can be 15:1, 16:1, 17:1, 18:1, 19:1, or 20:1. Before sintering the zirconia ceramic of the present invention, the silicon carbide fiber with an aspect ratio within this range carries the colorant, allowing the colorant to be fully dispersed in the overall slurry, providing a basis for stable color development. After sintering, it exhibits excellent toughness, density, hardness, and other properties together with the zirconia ceramic body material and additives.

[0047] Optionally, in the yttrium oxide-stabilized zirconia ceramic powder, the yttrium oxide content is 2.5-4% of the mass of the zirconia ceramic host material. In some specific examples, the yttrium oxide content is 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, or 4% of the mass of the zirconia ceramic host material.

[0048] Optionally, the colorant of the present invention is a cobalt metal salt that is easily soluble in water. That is, any cobalt metal salt that is easily soluble in water is within the scope of protection of the present invention. Further, the colorant includes cobalt chloride hexahydrate and cobalt chloride.

[0049] Optionally, the dispersant is one or more of ammonium polyacrylate, polyethylene glycol, ammonium polymethacrylate, and sodium tripolyphosphate; the lubricant is talc or polyvinyl alcohol; and the plasticizer is one or more of hydroxymethyl cellulose, polyvinyl alcohol, and bone glue.

[0050] Secondly, the second objective of this invention is to provide a method for preparing high-toughness zirconia ceramic, the technical features of which are as follows:

[0051] A method for preparing high-toughness gray zirconia ceramic includes the following preparation steps:

[0052] S1: The zirconia ceramic substrate material, dispersant, and pure water are mixed to form a slurry, and the slurry is ball-milled using zirconia beads until a first slurry with a D50 of 0.05μm to 0.25μm is formed. In some specific embodiments, D50 can be 0.05μm, 0.10μm, 0.15μm, 0.20μm, or 0.25μm. The mass of the zirconia ceramic substrate material accounts for 35-50% of the mass of the slurry. In some specific embodiments, the mass of the zirconia ceramic substrate material accounts for 35%, 40%, 45%, or 50% of the mass of the slurry.

[0053] S2: Add colorant to the first slurry, continue ball milling until the particle size inside the slurry tends to be uniform, then stop ball milling, adjust the slurry to be alkaline, stir evenly, and obtain color paste;

[0054] S3: Add composite additives to the color paste and disperse it fully using ultrasound. After standing for more than 24 hours, add plasticizer and lubricant and stir until it is evenly mixed to make the second paste.

[0055] S4: The second slurry is pressure spray dried using a pressure spray dryer, then dry-pressed, followed by debinding and sintering to obtain high-toughness gray zirconia ceramic; wherein the sintering temperature is 1250-1550℃, the sintering time is 1-4h, and the sintering atmosphere is a reducing atmosphere.

[0056] Optionally, in step S2, the pH value of the slurry is 9-12, and the pH value of the slurry only needs to be between 9 and 12.

[0057] Optionally, in step S3, the composite additive needs to be pretreated. The pretreatment step includes dispersing the composite additive in a 2-8 mol / L nitric acid solution. In some specific embodiments, the concentration of the nitric acid solution can be 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, or 8 mol / L. The temperature is controlled between 40-60°C. After soaking for 8-16 hours, the additive is rinsed with clean water and dried.

[0058] Optionally, in step S4, the reducing atmosphere is a high-purity hydrogen atmosphere, and during the sintering process, the hydrogen flow rate is controlled to be 0.5-1 L / min. In some specific embodiments, the hydrogen flow rate can be 0.5 L / min, 0.6 L / min, 0.7 L / min, 0.8 L / min, 0.9 L / min, or 1 L / min.

[0059] The gray zirconia ceramic of this invention is mainly achieved through the coloring reaction of cobalt. Cobalt metal salt is used as a colorant, which can be co-fired with zirconia ceramic and maintains stable color even after sintering and returning to room temperature. When cobalt metal salt is added to the first slurry, it exists in the form of cobalt ions, at which point the slurry appears pale pink. After adjusting the slurry to be alkaline, the overall color slurry turns blue or cyan, presumably because the cobalt ions exist in the form of cobalt hydroxide precipitate. Finally, during the sintering process, under a reducing atmosphere and with the synergistic effect of additives such as dispersants, lubricants, plasticizers, and composite auxiliaries, the sintered zirconia ceramic exhibits a stable gray color and possesses high toughness and other physicochemical properties.

[0060] Specifically, the color development principle of gray zirconia ceramics is as follows:

[0061] CoCl₂ + NaOH = Co(OH)Cl + NaCl

[0062] Co(OH)Cl+NaOH=Co(OH)2↓+NaCl

[0063] Ultimately, under the action of a reducing atmosphere, Co(OH)2 is reduced to Co metal, which makes the zirconia ceramic material stably gray. The range of the lab values ​​is 25≤L≤40, -1≤a≤0, and -2≤b≤1.

[0064] The present invention will be further described in detail below with reference to specific embodiments. Unless otherwise specified, all raw materials used in the following embodiments are commercially available products.

[0065] Example 1

[0066] A high-toughness gray zirconia ceramic comprises the following components:

[0067] Yttrium oxide stabilized zirconia ceramic powder, wherein the yttrium oxide content is 2.5% of the mass of the zirconia ceramic matrix material;

[0068] The colorant used is cobalt chloride hexahydrate, and the amount of colorant used is 2.0% of the amount of zirconium oxide ceramic main material.

[0069] Ammonium polyacrylate was selected as the dispersant, and its dosage was 1.5% of the amount of zirconium oxide ceramic main material.

[0070] The lubricant used is talc powder, and its dosage is 1.1% of the total amount of zirconia ceramic main material.

[0071] The plasticizer used is hydroxymethyl cellulose, and its dosage is 3.5% of the amount of zirconium oxide ceramic main material.

[0072] The composite additive is silicon carbide fiber with an aspect ratio of 15:1, and the amount of silicon carbide used is 0.65% of the amount of zirconia ceramic main material.

[0073] The specific preparation method includes the following preparation steps:

[0074] S1: The zirconia ceramic substrate material, dispersant and pure water are mixed to form a slurry, and the slurry is ball-milled until a first slurry with a D50 of 0.20 μm is formed, wherein the mass of the zirconia ceramic substrate material accounts for 35% of the mass of the slurry;

[0075] S2: Add colorant to the first slurry, continue ball milling until the particle size inside the slurry tends to be uniform, then stop ball milling, adjust the pH value of the slurry to 10, stir evenly, and obtain color paste;

[0076] S3: Add composite additives to the color paste and disperse it fully using ultrasound. After standing for more than 24 hours, add plasticizer and lubricant and stir until it is evenly mixed to make the second paste.

[0077] S4: The second slurry is subjected to pressure spray drying, dry pressing, debinding, and sintering to obtain high-toughness gray zirconia ceramic; wherein the sintering temperature is 1400-1550℃, the sintering time is 3-4h, the sintering atmosphere is high-purity hydrogen atmosphere, and the hydrogen flow rate is controlled at 0.8L / min during sintering to obtain the high-toughness gray zirconia ceramic of this application.

[0078] Example 2

[0079] A high-toughness gray zirconia ceramic comprises the following components:

[0080] Yttrium oxide stabilized zirconia ceramic powder, wherein the yttrium oxide content is 3% of the mass of the zirconia ceramic main material;

[0081] Cobalt chloride is selected as the colorant, and the amount of colorant used is 1.5% of the amount of zirconium oxide ceramic main material.

[0082] The dispersant used is polyethylene glycol, and the dosage is 1% of the amount of the zirconium oxide ceramic main material.

[0083] Polyvinyl alcohol is selected as the lubricant, and its dosage is 1.5% of the amount of zirconia ceramic main material.

[0084] Polyvinyl alcohol is selected as the plasticizer, and its dosage is 5.5% of the amount of zirconium oxide ceramic main material.

[0085] The composite additive is silicon carbide fiber with an aspect ratio of 20:1, and the amount of silicon carbide used is 0.25% of the amount of zirconia ceramic main material.

[0086] The specific preparation method includes the following preparation steps:

[0087] S1: The zirconia ceramic substrate material, dispersant and pure water are mixed to form a slurry, and the slurry is ball-milled until a first slurry with a D50 of 0.05 μm is formed, wherein the mass of the zirconia ceramic substrate material accounts for 45% of the mass of the slurry.

[0088] S2: Add colorant to the first slurry, continue ball milling until the particle size inside the slurry tends to be uniform, then stop ball milling, adjust the pH value of the slurry to 12, stir evenly, and obtain color paste;

[0089] S3: Add composite additives to the color paste and disperse it fully using ultrasound. After standing for more than 24 hours, add plasticizer and lubricant and stir until it is evenly mixed to make the second paste.

[0090] S4: The second slurry is subjected to pressure spray drying, dry pressing, debinding, and sintering to obtain high-toughness gray zirconia ceramic; wherein the sintering temperature is 1400-1550℃, the sintering time is 3-4h, the sintering atmosphere is high-purity hydrogen atmosphere, and the hydrogen flow rate is controlled at 1L / min during sintering to obtain the high-toughness gray zirconia ceramic of this application.

[0091] Example 3

[0092] A high-toughness gray zirconia ceramic comprises the following components:

[0093] Yttrium oxide stabilized zirconia ceramic powder, wherein the yttrium oxide content is 4% of the mass of the zirconia ceramic main material;

[0094] The colorant used is cobalt chloride hexahydrate, and the amount of colorant used is 2.5% of the amount of zirconium oxide ceramic main material.

[0095] The dispersants selected are ammonium polymethacrylate and sodium tripolyphosphate, and the dosage is 3% of the amount of zirconium oxide ceramic main material.

[0096] Polyvinyl alcohol is selected as the lubricant, and its dosage is 0.5% of the amount of zirconia ceramic main material.

[0097] The plasticizer is selected from hydroxymethyl cellulose and bone glue, and its dosage is 1.0% of the dosage of the zirconium oxide ceramic main material;

[0098] The composite additive is silicon carbide fiber with an aspect ratio of 18:1, and the amount of silicon carbide used is 1.25% of the amount of zirconia ceramic main material.

[0099] The specific preparation method includes the following preparation steps:

[0100] S1: The zirconia ceramic substrate material, dispersant and pure water are mixed to form a slurry, and the slurry is ball-milled until a first slurry with a D50 of 0.25 μm is formed, wherein the mass of the zirconia ceramic substrate material accounts for 50% of the mass of the slurry.

[0101] S2: Add colorant to the first slurry, continue ball milling until the particle size inside the slurry tends to be uniform, then stop ball milling, adjust the pH value of the slurry to 9, stir evenly, and obtain color paste;

[0102] S3: Add composite additives to the color paste and disperse it fully using ultrasound. After standing for more than 24 hours, add plasticizer and lubricant and stir until it is evenly mixed to make the second paste.

[0103] S4: The second slurry is subjected to pressure spray drying, dry pressing, debinding, and sintering to obtain high-toughness gray zirconia ceramic; wherein the sintering temperature is 1400-1550℃, the sintering time is 3-4h, the sintering atmosphere is high-purity hydrogen atmosphere, and the hydrogen flow rate is controlled at 0.5L / min during sintering to obtain the high-toughness gray zirconia ceramic of this application.

[0104] Example 4

[0105] The difference between this embodiment and Embodiment 1 is that the silicon carbide fiber in this embodiment has been pretreated. The pretreatment step includes ultrasonically dispersing the silicon carbide fiber in an 8 mol / L nitric acid solution, controlling the temperature between 40-60°C, soaking for 8-16 hours, rinsing with clean water and drying.

[0106] In step S2, the sintering temperature is 1250-1400℃ and the sintering time is 1-3h.

[0107] Example 5

[0108] The difference between this embodiment and Embodiment 4 is that in this embodiment, the concentration of the pretreated nitric acid solution is 5 mol / L.

[0109] Example 6

[0110] The difference between this embodiment and Embodiment 4 is that in this embodiment, the concentration of the pretreated nitric acid solution is 2 mol / L.

[0111] Example 7

[0112] The difference between this embodiment and Embodiment 4 is that in this embodiment, the concentration of the pretreated nitric acid solution is 10 mol / L.

[0113] Example 8

[0114] The difference between this embodiment and embodiment 4 is that in this embodiment, the aspect ratio of the silicon carbide fiber is 10:1.

[0115] Example 9

[0116] The difference between this embodiment and embodiment 4 is that in this embodiment, the aspect ratio of the silicon carbide fiber is 30:1.

[0117] Comparative Example 1

[0118] The difference between this comparative example and Example 1 is that the content range of each component in this example is not within the component range claimed by this invention, as detailed below:

[0119] A high-toughness gray zirconia ceramic comprises the following components:

[0120] Yttrium oxide stabilized zirconia ceramic powder, wherein the yttrium oxide content is 2.5% of the mass of the zirconia ceramic matrix material;

[0121] The colorant used is cobalt chloride hexahydrate, and the amount of colorant used is 10% of the amount of zirconium oxide ceramic main material.

[0122] Ammonium polyacrylate was selected as the dispersant, and its dosage was 4% of the amount of the zirconium oxide ceramic main material.

[0123] The lubricant used is talc powder, and its dosage is 2% of the dosage of the zirconia ceramic main material.

[0124] The plasticizer used is hydroxymethyl cellulose, and the dosage is 0.5% of the amount of zirconium oxide ceramic main material.

[0125] The composite additive is silicon carbide fiber with an aspect ratio of 15:1, and the amount of silicon carbide used is 1.5% of the amount of zirconia ceramic main material.

[0126] The preparation method is the same as in Example 1.

[0127] Comparative Example 2

[0128] The difference between this comparative example and Example 1 is that the silicon carbide fiber in this example is replaced by an equal amount of carbon fiber.

[0129] Comparative Example 3

[0130] The difference between this comparative example and Example 1 is that no composite additives are added in this example.

[0131] Comparative Example 4

[0132] The difference between this comparative example and Example 1 is that in step S1, the slurry is not mixed and ball-milled, but directly mixed evenly to form the first slurry;

[0133] Comparative Example 5

[0134] In this comparative example and Example 1, in step S1, the mixed slurry is ball-milled until a first slurry with a D50 of 0.01 μm is formed;

[0135] Comparative Example 6

[0136] The difference between this comparative example and Example 1 is that in step S2, a colorant is added to the first slurry, and after mixing evenly, the slurry is directly adjusted to be alkaline. That is, the colorant is not ground together with the first slurry after being added.

[0137] Comparative Example 7

[0138] The difference between this comparative example and Example 1 is that, in step S2, the pH value of the slurry is set to 8.

[0139] Comparative Example 8

[0140] The difference between this comparative example and Example 1 is that, in step S2, the pH value of the slurry is set to 13.

[0141] Comparative Example 9

[0142] The difference between this comparative example and Example 1 is that cobalt hydroxide is used as the colorant.

[0143] Comparative Example 10

[0144] The difference between this comparative example and Example 1 is that cobalt oxide is used as the colorant.

[0145] Performance testing

[0146] Physicochemical testing: The high-toughness gray zirconia ceramics prepared in Examples 1-9 and Comparative Examples 1-10 were processed into test pieces with a thickness of 1.0 mm. Then, the gray zirconia ceramic test pieces were tested for flexural strength, fracture toughness, Vickers hardness and density using a universal testing machine, a Vickers hardness tester and a solid density meter, respectively.

[0147] Color detection: The high-toughness gray zirconia ceramics prepared in Examples 1-9 and Comparative Examples 1-10 were processed into test pieces with a thickness of 1.5 mm and polished on both sides until the smoothness Ra was less than 0.04. The processed ceramic pieces were placed in a Konica Minolta CM-3700A-U device for detection, with an F2 light source, an observer angle of 10°, and the SCI mode was used for testing.

[0148] Using the Lab value of a 1.5 mm thick test piece of high-toughness gray zirconia ceramic prepared in Example 1 as a benchmark, JNCD tests were performed on the 1.5 mm thick test pieces of high-toughness gray zirconia ceramic prepared in Examples 2-9 and Comparative Examples 1-10 using GS-1164 multi-angle spectrophotometers. When the JNCD value is less than 2, it indicates that the color difference is small.

[0149] Table 1. Performance test charts of the test pieces prepared in the examples and comparative examples.

[0150]

[0151]

[0152] As can be seen from the comparison of the test data of Examples 1-9 and Comparative Examples 1-10 in Table 1, the high-toughness zirconia ceramics prepared using the formulation and preparation process within the scope of this application exhibit excellent performance. The colorant can be co-fired with the zirconia ceramics and maintains stable color even after sintering and returning to room temperature. The density of the prepared zirconia ceramics is 6.28 g / cm³. 3 The Vickers hardness is 1250 kgf / mm². 2 The above three-point bending strength is higher than 1300MPa, the fracture toughness is higher than 12MPa / m, the lab value range is 25≤L≤40, -1≤a≤0, -2≤b≤1, and the JNCD value is less than 2, which means that the color difference is very small and there are no color spots or patches, low hardness and high brittleness.

[0153] During the sintering process of the ceramic materials in Example 4 and Example 1, the sintering temperature of Example 4 is lower, and the sintering can be completed in a shorter time, with stable color development and energy saving. Furthermore, it maintains excellent fracture toughness, hardness, and other properties. This indicates that the pretreated silicon carbide fibers, in addition to maintaining the toughening and reinforcing role of silicon carbide fibers, also reduce the sintering temperature of the ceramic materials and shorten the sintering time.

[0154] The high-toughness gray zirconia ceramic prepared by this invention has excellent properties. It can stably exhibit gray color after zirconia ceramic sintering and maintain high toughness while keeping high density, which meets and is applicable to more high-end applications of gray zirconia ceramic.

[0155] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0156] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims, and the specification can be used to interpret the content of the claims.

Claims

1. A high-toughness gray zirconia ceramic, comprising a zirconia ceramic main material and an additive; It is characterized in that The main material of the zirconia ceramic is yttria-stabilized zirconia ceramic powder; the additives include colorants, dispersants, lubricants, plasticizers and composite additives; The colorant is cobalt chloride hexahydrate or cobalt chloride, and the amount of the colorant is 1.5-2.5% of the amount of the zirconia ceramic main material; The amount of the dispersant is 1-3% of the amount of the zirconia ceramic main material; The amount of the lubricant is 0.5-1.5% of the amount of the zirconia ceramic main material; The amount of the plasticizer is 1.0-5.5% of the amount of the zirconia ceramic main material; The amount of the composite additive is 0.25-1.25% of the amount of the zirconia ceramic main material; The composite auxiliary agent needs to be pre-treated, and the pre-treatment step includes dispersing the composite auxiliary agent in a 2-8 mol / L nitric acid solution, controlling the temperature between 40-60° C., soaking for 8-16 hours, rinsing with clean water and drying; The composite auxiliary agent is silicon carbide fiber, and the aspect ratio of the silicon carbide fiber is in the range of 15:1-20:1; The method for preparing high-toughness gray zirconia ceramics comprises the following preparation steps: S1: Mixing a zirconia ceramic main material, a dispersant and pure water to form a mixed slurry, and ball-milling the mixed slurry until a first slurry with a D50 of 0.05 μm to 0.25 μm is formed, wherein the mass of the zirconia ceramic main material accounts for 35-50% of the mass of the mixed slurry; S2: adding a colorant to the first slurry, continuing ball milling until the particle size inside the slurry tends to be consistent, then stopping the ball milling, adjusting the pH value of the slurry to 9-12, stirring evenly, and obtaining a color paste; S3: adding composite additives to the color paste, and fully dispersing it by ultrasonic wave, and then standing for more than 24 hours, adding plasticizer and lubricant, and stirring until the mixture is evenly mixed to prepare the second slurry; S4: The second slurry is subjected to pressure spray drying, dry pressing, binder removal and sintering to obtain high-toughness gray zirconia ceramics; wherein the sintering temperature is 1250-1550°C, the sintering time is 1-4h, and the atmosphere during the sintering is a reducing atmosphere.

2. A high-toughness grey zirconia ceramic according to claim 1, It is characterized in that In the yttria-stabilized zirconia ceramic powder, the content of yttria is 2.5-4% of the mass of the zirconia ceramic main body material.

3. A high-toughness gray zirconia ceramic according to claim 1, It is characterized in that The dispersant is one or more of ammonium polyacrylate, polyethylene glycol, ammonium polymethacrylate, and sodium tripolyphosphate; the lubricant is talcum powder or polyvinyl alcohol; and the plasticizer is polyvinyl alcohol or gelatin.

4. A high-toughness grey zirconia ceramic according to claim 1, It is characterized in that In step S4, the reducing atmosphere is a high-purity hydrogen atmosphere, and during the sintering process, the gas flow rate of hydrogen is controlled to be 0.5-1 L / min.