A device and method for preparing perovskite film

Through the cooperation of the high-pressure and high-temperature film formation control device and the gas supply container, the uniformity and flatness of the perovskite film are achieved, solving the uniformity problem in the preparation of large-area films of perovskite solar cells, and improving battery performance and efficiency .

CN117779164BActive Publication Date: 2024-12-06BEI JING SHUO WEI GUANG DIAN KE JI YOU XIAN GONG SI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311718180.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-12-06
Estimated Expiration
2043-12-14

AI Technical Summary

Technical Problem

The prior art is difficult to achieve uniformity and flatness of large-area films in perovskite solar cells, and traditional processes such as slit coating, scraping coating and vacuum multi-source evaporation have problems with high energy consumption and equipment parameters dependence. , limiting the industrialization process of perovskite batteries.

Method used

A high-pressure and high-temperature film formation control device was designed to realize the film formation process of the film under the heating device by placing a large-area perovskite polycrystalline film in a closed container and combining the reaction gas provided by the gas supply container. The intermediate liquid phase state is transformed and recrystallized, reducing body phase defects, and improving film uniformity and flatness.

Benefits of technology

Through this device and method, a large-area ultra-thin perovskite single crystal thin film was obtained, which significantly improved the performance of perovskite solar cells, and the photoelectric conversion efficiency was greater than 20%, solving the film uniformity and flatness problems that cannot be achieved in traditional processes. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117779164B_ABST
    Figure CN117779164B_ABST
Patent Text Reader

Abstract

The present invention discloses a device and method for preparing a perovskite film, the device comprising: a film forming control container, a first heating device and a gas supply container, the film forming control container is provided with a horizontal placement area for placing a large-area perovskite polycrystalline film, and is also provided with an exhaust port that can be selectively connected to the atmosphere, and a precision gas valve is correspondingly provided at the exhaust port. The gas supply container is connected to the film forming control container through a connecting pipe, and the connecting pipe is also provided with a first opening and closing gas valve, and the connecting pipe or the film forming control container is also provided with a pressure detection device for detecting its internal pressure, and the gas supply container is also provided with an atmospheric communication conduit with a second switch valve. The device is based on the "solid-liquid-solid" perovskite film forming mechanism, and the intermediate phase transition time is regulated by a gas pressure-assisted recrystallization method to obtain a single crystal or single crystal-like large-area perovskite film, which minimizes the bulk phase defects and greatly improves the performance after being assembled into a device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optoelectronic functional materials and devices, and in particular to a device and method for preparing a perovskite film, a solar cell and a method for preparing the solar cell. Background Art

[0002] With the rapid progress of human society, environmental and energy issues under the background of sustainable development have become the focus of attention of all countries. The establishment of the "dual carbon" policy represents my country's determination to develop renewable clean energy. Photovoltaic technology, as the most widely used clean energy technology in the market, will become one of the focuses of future development. Up to now, monocrystalline silicon-based solar cells have occupied more than 95% of the photovoltaic market with their high efficiency and high stability, and have brought a very considerable supply of clean energy to my country. However, the high cost, long industrial chain and high energy consumption of upstream enterprises of silicon-based solar cells have limited their development speed. At the same time, the efficiency of silicon-based solar cells has gradually approached the theoretical limit (~29%) and has grown slowly in recent years. Therefore, it is very important to develop a new photovoltaic technology with low cost, high theoretical efficiency and simple manufacturing industry line.

[0003] Perovskite solar cells are a new type of photovoltaic technology with low cost and high theoretical efficiency (~31%). Since its research began in 2009, the photoelectric conversion efficiency of small-area cells in the laboratory has been close to 26%, which is comparable to the efficiency of silicon-based cells. Especially in the second half of 2021, the industrialization process of perovskite solar cells has accelerated, and early attempts at industrialization such as laboratory technology amplification, pilot production line construction, and sample display are in full swing. Among them, it is still very difficult to enlarge the common small-area cells in the laboratory to product-level large-area cells without affecting the efficiency and stability of the cells. At present, there is no special amplification process suitable for perovskites. Instead, the slit coating, scraping and other equipment commonly used in the traditional panel industry are used. The performance of industrialized large-area perovskite cells is still far behind the laboratory level. Therefore, the development of proprietary large-area process technologies for perovskite materials, films, and batteries is the key to achieving high-performance perovskite commercial components.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The object of the present invention is to provide a device and method for preparing a perovskite film, a solar cell and a method for preparing the solar cell, so as to improve the above technical problems.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a device for preparing a perovskite film, comprising:

[0008] The film formation control container is a closed container, and the film formation control container is provided with a horizontal placement area for placing a large-area perovskite polycrystalline film. The film formation control container is provided with an exhaust port that can be selectively connected to the atmosphere, and the exhaust port is correspondingly provided with a precision gas valve with controllable opening.

[0009] The first heating device is used to heat the placement area of ​​the film formation control container.

[0010] An air supply container is connected to a film forming control container via a connecting pipe, and a first opening and closing air valve is also provided on the connecting pipe. A pressure detection device for detecting the internal pressure of the film forming control container is also provided on the connecting pipe or the film forming control container. The air supply container is also provided with an atmospheric connecting conduit, and a second switching valve is provided on the atmospheric connecting conduit.

[0011] In a second aspect, the present invention also provides a method for preparing a large-area perovskite single crystal thin film using the above-mentioned device, which comprises:

[0012] a. Place the large-area perovskite polycrystalline film in the horizontal placement area of ​​the film formation control container and close the precision valve.

[0013] b. Turn on the first heating device, adjust the heating temperature to the preset film forming temperature, open the first on-off gas valve, continuously input the reaction gas to the preset film forming pressure through the gas supply container to the film forming control container, and the large-area perovskite polycrystalline film becomes an intermediate liquid phase state, and close the first on-off gas valve.

[0014] c. After confirming that the pressure in the film forming control container is stable, open the precision air valve, exhaust to atmospheric pressure, and control the exhaust time to 3min~5h.

[0015] d. Control the first heating device to maintain the annealing temperature for annealing.

[0016] In a third aspect, the present invention also provides a method for preparing a solar cell, which comprises: performing interface post-processing optimization on the large-area perovskite single crystal film prepared by the above method, and then preparing a top transmission layer on the optimized large-area perovskite single crystal film, and then preparing a top electrode on the top transmission layer.

[0017] In a fourth aspect, the present invention further provides a solar cell, which is prepared by the above-mentioned method for preparing a solar cell, and the photoelectric conversion efficiency of the solar cell is greater than 20%.

[0018] The present invention has the following beneficial effects: by constructing and designing a high-pressure and high-temperature film-forming control device for perovskite, based on the "solid-liquid-solid" perovskite film-forming mechanism, by placing a large-area perovskite polycrystalline film in a film-forming control container, and then combining a gas supply container to supply gas to the film-forming control container, the large-area perovskite polycrystalline film can be transformed from a polycrystalline film to an intermediate liquid phase state under the temperature provided by the first heating device and the pressure of the reaction gas provided by the gas supply container, and then the intermediate phase transition time is regulated under the gas pressure-assisted recrystallization method to obtain a single crystal or single crystal-like large-area perovskite film, which minimizes bulk defects and greatly improves the performance after being assembled into a device. And because the thickness of the initial polycrystalline film is determined, the thickness of the film finally grown does not change much, which provides an effective process idea for the preparation of large-area ultra-thin perovskite single crystal films. Compared with traditional slit coating, blade coating, vacuum multi-source evaporation and other processes, the device and method of the present invention controls the recrystallization and regrowth of the film by uniform high-pressure gas, which will greatly improve the uniformity of the film and achieve film uniformity and flatness that cannot be obtained by traditional solution processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0020] Figure 1 A schematic diagram of the structure of a device for preparing a perovskite film according to an embodiment of the present invention;

[0021] Figure 2 Schematic diagram of the process of converting a large-area perovskite polycrystalline thin film into a large-area perovskite single crystal thin film according to an embodiment of the present invention;

[0022] Figure 3 The perovskite cell based on single crystal thin film in Example 1 J - V curve.

[0023] Icons: 100-device for preparing perovskite film; 101-precision gas valve; 102-second opening and closing gas valve; 103-first opening and closing gas valve; 104-third opening and closing gas valve; 110-film formation control container; 111-exhaust duct; 112-first atmosphere connecting duct; 113-connecting pipe; 114-pipeline temperature control device; 115-pressure detection device; 116-connector; 120-first heating device; 130-gas supply container; 131-second atmosphere connecting duct; 140-second heating device; 150-large-area perovskite polycrystalline film; 151-intermediate liquid phase; 160-gas generating material; 170-large-area perovskite single crystal film; 210-transparent conductive substrate; 220-bottom transmission layer. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0025] The following specifically describes a device and method for preparing a perovskite film, a solar cell, and a method for preparing a solar cell provided by the present invention.

[0026] At present, the existing and popular methods for preparing large-area perovskite films in the laboratory or industrialized large-area perovskite films include slit coating, blade coating, and vacuum multi-source evaporation. The commonly used slit coating and blade coating methods control the crystallization of the film by controlling the solution, and the film forming speed is relatively fast. It is currently difficult to solve the problem of uniformity of large-area films; the vacuum multi-source evaporation method is an effective process route to solve the uniformity problem, but this method is highly energy-consuming and heavily dependent on equipment parameters. At the same time, the gas phase of perovskite still faces major problems. It is difficult to obtain high-quality perovskite films, which is an important factor restricting its development. In view of this, the present invention creatively proposes the following solution.

[0027] See attached Figure 1 Some embodiments of the present invention provide a device 100 for preparing a perovskite thin film, which includes: a film formation control container 110, a first heating device 120, a gas supply container 130 and a second heating device 140.

[0028] Specifically, the film formation control container 110 is a sealed container, and the film formation control container 110 is provided with a horizontal placement area for placing a large-area perovskite polycrystalline film 150. Generally speaking, the horizontal placement area is the bottom wall of the film formation control container 110. The film formation control container 110 can be provided with an upper cover (not shown), and the upper cover and the body can be opened and closed by detachable or transfer methods to achieve the placement and removal of the perovskite film. It should be noted that the connection between the upper cover and the body should be provided with a sealing structure to achieve that when the film formation control container 110 is closed, the inside of the film formation control container 110 is in a sealed state.

[0029] Furthermore, the film formation control container 110 can be a high pressure container made of common heat conductive materials such as stainless steel, and its shape and size are not limited. The first heating device 120 is used to heat the placement area of ​​the film formation control container 110. The first heating device 120 includes but is not limited to an oil bath pot, which can achieve uniform heating of the inside of the film formation control container 110. The film formation control container 110 is placed in a common oil bath pot for temperature control, and the immersion height needs to reach more than 80% of the entire film formation control container 110, so as to ensure the temperature of the film formation control container 110 is stable.

[0030] Furthermore, the film formation control container 110 is provided with an exhaust port that can be selectively connected to the atmosphere, and the exhaust port is correspondingly provided with a precision gas valve 101 with controllable opening. In some embodiments, an exhaust duct 111 connected to the atmosphere is provided at the exhaust port, and the precision gas valve 101 is provided on the exhaust duct 111, and the exhaust duct 111 is detachably connected or integrally connected to the body of the film formation control container 110. In other embodiments, an exhaust port can also be directly opened on the film formation control container 110, and a precision gas valve 101 is designed at the exhaust port to achieve sealing or exhaust. It should be noted that the precision gas valve 101 includes but is not limited to a needle valve, a regulating valve, a diaphragm valve or a ball valve, and the precision gas valve 101 is a high-pressure valve.

[0031] In some embodiments, the film formation control container 110 is further provided with a first atmosphere communication conduit 112 connected to the atmosphere, and the first atmosphere communication conduit 112 is further provided with a second on-off gas valve 102. The first atmosphere communication conduit 112 can be used to discharge internal gas before the reaction, and gas can be introduced after the reaction to discharge the remaining reaction gas in the film formation control container 110 from the exhaust conduit 111.

[0032] See again Figure 1The gas supply container 130 is connected to the film forming control container 110 through the connecting pipe 113, and the connecting pipe 113 is also provided with a first opening and closing gas valve 103. The gas supply container 130 can be a high-pressure resistant container made of common materials such as glass and stainless steel, and the inner wall of the container is coated with a high-temperature resistant and corrosion-resistant coating, such as a polytetrafluoroethylene coating. The gas supply container 130 is also provided with a second atmosphere communication conduit 131, and the second atmosphere communication conduit 131 is provided with a third opening and closing gas valve 104.

[0033] For reference, the gas supply container 130 contains a gas generating material 160, and the gas generating material 160 includes but is not limited to a liquid capable of generating amine gas, alcohol gas or water vapor, for example, an aqueous solution of methylamine, a tetrahydrofuran solution of methylamine, a methanol solution of methylamine, an aqueous solution of pyridine, etc., common amines such as methylamine, methylamine, pyridine, ammonia, and H 2 O, methanol and other gases. The second heating device 140 is arranged outside the gas supply container 130, and is used to heat the gas supply container 130. For example, the second heating device 140 is an oil bath pot, and the gas supply container 130 is placed in a common oil bath pot for temperature control. The immersion height needs to reach more than 80% of the entire gas supply container 130, so as to ensure the temperature stability in the gas supply container 130. When the oil bath pot is heated, the gas in the generating solution will continuously overflow from the solution, and the gas pressure in the film forming control container 110 will continue to increase until it reaches the maximum value of dynamic equilibrium.

[0034] Furthermore, the connecting pipe 113 needs to realize temperature control to ensure that the gas does not condense into liquid in the connecting pipe 113 due to low temperature and affect the reaction. That is, the outer wall of the connecting pipe 113 is provided with a pipe temperature control device 114. For example, the pipe temperature control device can use a heat-conducting metal material to realize electrical metal heat conduction temperature control, or use an external liquid heat transfer method to control the temperature. In some embodiments, in order to facilitate installation, disassembly and transportation, the connecting pipe 113 can be divided into two parts. During installation, they are connected together by a connector 116, and when they need to be disassembled, the connector 116 is removed to achieve separation.

[0035] In some embodiments, the device 100 for preparing a perovskite film is also provided with a pressure detection device 115 for detecting the internal air pressure of its film formation control container 110, for example, the pressure detection device is a pressure detection gauge. The pressure detection device 115 can be arranged on a connecting pipe 113 connected to the film formation control container 110, and is located on the connecting pipe 113 between the first opening and closing air valve 103 and the film formation control container 110. Of course, in other embodiments, the pressure detection device 115 can also be arranged on the part where the first atmosphere communication conduit 112 is connected to the film formation control container 110, or on a separate pipeline outside the film formation control container 110 for detecting its internal pressure. The pressure detection device 115 is responsible for real-time detection of pressure changes in the entire communication system or the film formation control container 110, and the precision air valve 101 is used to control the changes in air pressure in the entire system or the film formation control container 110.

[0036] It should be noted that the valves in the embodiments of the present invention are all high-pressure valves. In addition, in some embodiments, the gas supply container 130 may not contain the second heating device 140, and the gas generating material 160 may not be contained therein. The second atmosphere communication conduit 131 may be directly connected to a gas source device (such as an amine gas cylinder, etc.) to provide the film forming control container 110 with the corresponding high-pressure gas.

[0037] In combination with the above devices, a large-area perovskite polycrystalline film 150 can be placed in a film-forming control container 110, and a preset film-forming temperature for phase change transformation is provided to the film-forming control container 110 through the first heating device 120. Then, the gas supply container 130, under the action of the second heating device 140, causes the gas generating material 160 to generate gas and enter the film-forming control container 110. After reaching the preset film-forming pressure, the polycrystalline film is converted into an intermediate liquid phase state, and then the intermediate phase transition time is regulated by the recrystallization method assisted by gas pressure to obtain a single crystal or quasi-single crystal large-area perovskite film.

[0038] It should be noted that the large-area perovskite polycrystalline film 150 mentioned in each embodiment of the present invention refers to a film with an area greater than 10 cm 2 of polycrystalline perovskite thin films.

[0039] Some embodiments of the present invention also provide a method for preparing a large-area perovskite single crystal film 170 using the above-mentioned device, which comprises:

[0040] S1. Place the large-area perovskite polycrystalline film 150 in the horizontal placement area of ​​the film formation control container 110 and close the precision gas valve 101.

[0041] Specifically, in some embodiments, the horizontal placement area of ​​the film formation control container 110 is the bottom wall of the film formation control container 110. The large-area perovskite polycrystalline film 150 is first prepared on a substrate material, and then the substrate material is placed in the film formation control container 110, for example, Figure 2 The large-area perovskite polycrystalline film 150 covers the bottom transmission layer 220, and the bottom transmission layer 220 is combined with the transparent conductive substrate 210. The bottom transmission layer 220 is an electron transmission layer or a hole transmission layer. The electron transmission layer can be made of titanium oxide (TiO2), zinc oxide (ZnO), tin oxide (SnO 2 ), any one of nickel oxide, magnesium oxide, copper oxide, cuprous oxide, and tungsten oxide; the hole transport layer can be made of organic and inorganic materials, and organic materials include but are not limited to: Spiro-OMeTAD, PEDOT:PSS, TPD, PTAA, P3HT, PCPDTBT and other organic P-type semiconductor materials; inorganic materials include but are not limited to: Ni x O.V 2 O 5 、CuI、MoO 3 , CuO, Cu 2 O and other inorganic P-type semiconductor materials. An appropriate amount of bis(trifluoromethane)sulfonyl imide lithium salt and 4-tert-butylpyridine (4-tBP) are commonly used to dope the organic hole transport layer. The selection of the electron and hole transport layers depends on whether the final battery component is formal or trans. For mesoporous perovskite solar cells, the metal oxide mesoporous layer can be made of TiO 2 The slurry is sintered.

[0042] The transparent conductive substrate 210 is first thoroughly cleaned and treated with UV and / or ozone, and the bottom transmission layer 220 can be deposited by solution spin coating, physical vapor deposition (PVD), etc. If a large-area component is subsequently prepared, the transparent conductive substrate 210 needs to be laser-scribed and the bottom transmission layer 220 needs to be patterned before being placed in the film formation control container 110.

[0043] It should be noted that the large-area perovskite polycrystalline film 150 deposited on the bottom transmission layer 220 can be deposited by common perovskite film deposition methods such as solution spin coating, slit coating, blade coating, vacuum vapor evaporation, chemical vapor deposition (CVD), etc., requiring the perovskite film to completely cover the transparent conductive substrate 210. The transparent conductive substrate 210 can be replaced by common silicon cell substrates such as HJT, TOPCon, and PERC.

[0044] In some embodiments, the perovskite polycrystalline film may be selected from the general chemical formula ABX 3 A is CH 3 NH 3+ (MA + ), NH 2 =CHNH 2 + (FA + ), C 4 H 9 NH 3 + , Cs + , Rb + One or a mixture of 2+ , Sn 2+ ,Ge 2+ , Sb 3+ 、Bi 3+ 、Ag + 、Au 3+ 、Ti 4+ At least one of; X is Cl - ,Br - , I - Or one or a mixture of halogen-like elements.

[0045] It should be noted that the size of the polycrystalline film will depend on the area of ​​the final perovskite battery component, and the size of the film formation control container 110 can also be adjusted and enlarged accordingly according to the required area of ​​the final component.

[0046] In some embodiments, the transparent conductive substrate (substrate) corresponding to the large-area perovskite polycrystalline film 150 in the film formation control container can be made of transparent materials such as glass and flexible plastic. The transparent electrode material can be indium tin oxide (ITO), fluorine-doped tin oxide (FTO), aluminum-doped zinc oxide (AZO), silver nanowires, graphene or carbon nanotubes. One of ITO conductive glass, FTO conductive glass, AZO conductive glass, silver nanowire-modified conductive glass, graphene-modified conductive glass and carbon nanotube layer-modified conductive glass is often used as a transparent substrate and a transparent electrode.

[0047] Before closing the precision gas valve 101, check the high pressure gas sealing condition of the closed system, with N 2 The filling method increases the air pressure in the device and makes the pressure display reach the pressure required for the experiment. At the same time, the device is sealed for 10 minutes to observe whether the pressure display changes significantly. And a proper amount of N is continuously injected into the communication system through the second atmosphere communication conduit 131. 2 To exhaust the uncertain factors such as air and water vapor inside the device to ensure a pure inert atmosphere inside the device.

[0048] S2, start the first heating device 120, adjust the heating temperature to the preset film forming temperature, open the first on-off gas valve 103, continuously input the reaction gas to the film forming control container 110 through the gas supply container 130 to the preset film forming pressure, and the large-area perovskite polycrystalline film 150 turns into the intermediate liquid phase 151 (see Figure 2 ), close the first on-off air valve 103.

[0049] In some embodiments, the preset film forming temperature is 60 o C~250 o C, for example 60 o C. 70 o C. 80 o C. 90 o C. 100 o C. 120 o C. 150 o C. 160 o C. 180 o C. 200 o C. 230 o C. 240 o C or 250 o C, etc.; the preset pressure for film formation is 0.01~0.50 MPa, such as 0.05MPa, 0.1MPa, 0.2MPa, 0.25MPa, 0.3MPa, 0.35MPa, 0.4MPa, 0.45MPa or 0.5MPa, etc.

[0050] Specifically, the reaction gas is continuously input into the film forming control container through the gas supply container to the preset film forming pressure: a gas generating material capable of generating reaction gas is added to the gas supply container, the gas generating material in the gas supply container is heated, and the reaction gas overflows into the film forming control container through the connecting pipe. When setting the temperature of the oil bath pot of the entire device, it should be ensured that the temperature control of the oil bath pot of the gas generating device starts last, and before the gas overflows, it should be ensured that the temperature of the film forming control container 110 and the connecting pipe 113 has reached the preset temperature and remains stable. Among them, the lowest setting insulation temperature of the entire device shall not be lower than the condensation temperature of the reaction gas.

[0051] The gas-bound perovskite intermediate phase is a liquid or quasi-liquid with a certain viscosity. For example, the chemical formula of the intermediate phase may be CH 3 NH 3 PbI 3 MA. For different perovskite film components and different reaction gases, the best stabilization time under the maximum gas pressure is adjusted, that is, the closing reaction time of the first on-off gas valve 103 is about 5-20 minutes, at which time the color or morphology of the perovskite film will change significantly.

[0052] S3. After confirming that the pressure in the film forming control container 110 is stable, open the precision gas valve 101 to exhaust to atmospheric pressure, and control the exhaust time to 3 minutes to 5 hours.

[0053] Specifically, by observing whether the reading of the pressure detection device 115 is stable, for example, if there is a change inside within 5 minutes, the precision gas valve 101 is opened to discharge the gas in the film forming control container 110, and the air pressure in the device is continuously reduced until it is fully connected to the atmosphere.

[0054] S4, controlling the first heating device to maintain the annealing temperature for annealing.

[0055] Specifically, in some embodiments, the annealing temperature is 70 o C~250 o C, for example 80 o C. 90 o C. 100 o C. 110 o C. 120 o C. 130 o C. 140 o C. 150 o C. 160 o C. 170 o C. 180 o C. 190 o C. 200 o C. 210 o C. 220 o C. 230 o C or 240 o C, etc., and the annealing time is 10min~60min, such as 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min, etc. By adjusting the balance between the film annealing temperature and the ambient gas pressure, the rate of gas overflow / volatilization from the intermediate phase film can be controlled, and the kinetic process of film recrystallization from the intermediate phase can be adjusted, so as to finally obtain a single crystal or quasi-single crystal film with almost no bulk defects.

[0056] In some embodiments, step S5 is further included, wherein the large-area perovskite single crystal film 170 obtained after annealing is taken out and naturally cooled at room temperature to form an oxide layer on the surface to passivate surface defects.

[0057] At the same time as step S5 is performed, the large-area perovskite single crystal film 170 is taken out and replaced with another large-area perovskite polycrystalline film 150 that needs to be reacted, and the air is re-exhausted and the first on-off valve 103 is opened to connect the two devices so that the next single crystal film can be grown.

[0058] It should be noted that the film forming control container 110 replaced with a new perovskite film can be disassembled separately, and then the film forming control container 110 can be exhausted by controlling the first on-off gas valve 103 using the high-pressure gas of the gas supply container 130 to ensure that the growth atmosphere of each perovskite film is the same, thereby improving repeatability. In the workflow of preparing a perovskite single crystal film by a high-pressure and high-temperature film forming device, the gas used for the exhaust step includes but is not limited to N 2 , O 2 , H 2 One or more gases, etc., should be selected according to the specific requirements based on the components of the perovskite film.

[0059] Furthermore, some embodiments of the present invention also provide a method for preparing a solar cell, comprising:

[0060] (1) Performing post-processing optimization on the interface of the large-area perovskite single crystal film 170 prepared by the above method. Specifically, the surface of the perovskite single crystal film usually needs to be post-processed and optimized by solution spin coating, vacuum evaporation, etc. to treat surface defects, wherein common post-processing materials are one or more materials such as ammonium salts, amine small molecules, fullerenes, polymers, etc.

[0061] (2) Preparing a top transport layer on the optimized large-area perovskite single crystal film 170. The top transport layer can be made of the above-mentioned common electron or hole transport layer materials, and the preparation method can adopt solution spin coating, blade coating, slit coating, vacuum thermal deposition, chemical vapor deposition and other process technologies.

[0062] (3) Prepare the top electrode on the top transport layer. The top electrode can be made of metals such as Au, Ag, and Cu, and is prepared by vacuum thermal evaporation. In order to rationally utilize the battery area and facilitate testing, templates of different shapes are often used to control the shape of the top electrode.

[0063] Some embodiments of the present invention further provide a solar cell, which is prepared by the above-mentioned method for preparing a solar cell, and the photoelectric conversion efficiency of the solar cell is greater than 20%.

[0064] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0065] Example 1

[0066] This embodiment 1 adopts Figure 1 The device 100 for preparing a perovskite film is used to prepare a large-area perovskite single crystal film 170, and the specific operations are as follows:

[0067] In the first step, the ITO glass substrate was ultrasonically cleaned with deionized water, acetone, optical glass cleaner, deionized water, and isopropanol in sequence, and then dried in an oven at 60°C for 6 h. Then, a 5 wt% SnO2 solution was spin-coated on the ITO surface. 2 Nanoparticle dispersion, wherein the solvent used is distilled water. The spin coating speed is 3000 rpm, the spin coating time is 20 s, and the acceleration is 2000 rpm / s. The substrate is then heated and annealed at 150° C. for 30 min.

[0068] The second step is to add SnO 2 Transfer the film substrate to N 2 In the atmosphere glove box, 1.3 mol / L perovskite precursor solution was loaded on SnO 2 The spin coating speed is 6000 rpm, the spin coating time is 10 s, and the acceleration is 2000 rpm / s. The formula of the perovskite precursor solution is: the chemical composition is FAPbI 3 The perovskite was dissolved in a mixed solvent of DMF and DMSO (V / V=9:1). After the spin coating, the precursor film was transferred to a heating stage and annealed at 150°C for 5 min.

[0069] The third step is to wait for the film (Poly-FAPbI 3 ) is cooled and placed at the bottom of the film forming control container 110 of the device 100 for preparing a perovskite thin film, and 50 mL of pyridine solution (Py, 99.5%) is placed in the gas supply container 130 and the entire system is sealed. Then, the second atmosphere communication conduit 131 connecting the gas supply container 130 to the air is connected to the high pressure N 2 Connect and open all valves of the whole device to make N 2 Fill the entire device, about 1min of N 2 After the injection, close all valves and cut off the connection with high pressure N 2 connectivity.

[0070] The fourth step is to heat the oil bath on one side of the film forming control container 110 to 150°C and ensure that the height of the oil bath reaches 80% of the height of the film forming control container 110. At the same time, the pipeline temperature control device 114 is set to 150°C. This process takes about 3 minutes. Then adjust the oil bath on one side of the gas supply container to 150°C. At this time, you can open the first on-off valve 103 and ensure that the other valves connected to the atmosphere are closed. Observe the indication of the pressure detection device 115 until it stabilizes, and observe that the color of the perovskite film completely turns into a transparent white state (intermediate state, FAPbI 3 Py), at this time, the whole device system is kept stable for 10 minutes.

[0071] Step 5: Then close the first on-off air valve 103 and observe whether the reading of the pressure detection device 115 is stable within 5 minutes. If it is stable, adjust the precision air valve 101 of the film forming control container 110 to release the pyridine gas in the film forming control container 110. This decompression and degassing process needs to last for 10 minutes. During this process, observe the pressure detection device 115 at all times to grasp the decompression progress. 3 The perovskite film gradually undergoes gas desorption and regenerates from a transparent white intermediate film to FAPbI 3 Single crystal thin film (SC-FAPbI 3 ,See Figure 2 ). When the pressure detection device 115 indicates that the pressure is at normal pressure, close the precision gas valve 101 connecting the film forming control container 110 to the outside world and continue heating at 150 degrees for 5 minutes.

[0072] Step 6: SC-FAPbI 3 The film was taken out and cooled naturally at room temperature. This process is to form an oxide layer on the surface to passivate surface defects. 3 The film was transferred to a glove box, and a chlorobenzene solution of 72.3 mg / mL Spiro-OMeTAD was spin-coated on the perovskite single crystal film, and each milliliter of the solution contained 17.5 μL of lithium salt (520 mg / mL dissolved in acetonitrile) and 28.8 μL of 4-tBP. The spin coating speed was 4000 rpm and the spin coating time was 25 s. After the film was formed, 80 nm thick gold was evaporated as the metal top electrode. The photoelectric conversion efficiency of the cell can reach 24% (see Figure 3 ).

[0073] Example 2

[0074] The only difference between this embodiment and embodiment 1 is that in the second step, the perovskite component is replaced with MAPbI 3 , the gas generating material is replaced with a tetrahydrofuran solution of methylamine, and the three annealing and insulation temperatures in the device are all set to 100 degrees, and MAPbI can be grown according to the corresponding method 3 The single crystal or quasi-single crystal film finally achieved a photoelectric conversion efficiency of 22% for solar cells based on this perovskite.

[0075] Example 3

[0076] The only difference between this embodiment and Embodiment 1 is that, in the first step, the bottom transport layer is replaced by a PTAA hole transport layer, and subsequently the top transport layer is replaced by a C60 electron transport layer, and the metal electrode is replaced by a Cu electrode to prepare an inverse perovskite solar cell, whose photoelectric conversion efficiency reaches 23%.

[0077] Example 4

[0078] The only difference between this embodiment and embodiment 1 is that in the first step, the transparent conductive substrate is replaced with a flexible PET / ITO transparent conductive substrate, and the photoelectric conversion efficiency of the perovskite solar cell prepared based on this substrate reaches 22%.

[0079] In summary, the device of the embodiment of the present invention can be proportionally enlarged to meet the preparation of large-area perovskite films and components, solving the problem of large-area uniformity, and also providing an effective process idea for realizing large-area ultra-thin perovskite single crystals. This device and method are the first in the research field of perovskite solar cells. The perovskite film grown using this device and method will be able to achieve ultra-large-area ultra-thin perovskite single crystals in the industry, making perovskite single crystal cells and components possible.

[0080] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a large-area perovskite single crystal thin film, characterized in that: The film is prepared by using a device for preparing a perovskite film, which comprises: a film formation control container, a first heating device and a gas supply container, wherein the film formation control container is a closed container, and the film formation control container is provided with a horizontal placement area for placing a large-area perovskite polycrystalline film, and the film formation control container is provided with an exhaust port that can be selectively connected to the atmosphere, and the exhaust port is correspondingly provided with a precision gas valve with a controllable opening; the first heating device is used to heat the placement area of ​​the film formation control container; the gas supply container is connected to the film formation control container through a connecting pipe, and the connecting pipe is also provided with a first opening and closing gas valve, and the connecting pipe or the film formation control container is also provided with a pressure detection device for detecting the internal pressure of the film formation control container, and the gas supply container is also provided with an atmospheric communication conduit, and the atmospheric communication conduit is provided with a second switch valve; The method for preparing a large-area perovskite single crystal film includes: a. placing a large-area perovskite polycrystalline film in the horizontal placement area of ​​the film formation control container and closing the precision gas valve; b. Turn on the first heating device, adjust the heating temperature to the preset film forming temperature, open the first on-off gas valve, continuously input the reaction gas to the preset film forming pressure through the gas supply container to the film forming control container, and the large-area perovskite polycrystalline film becomes an intermediate liquid phase state, and close the first on-off gas valve; c. After confirming that the pressure in the film forming control container is stable, open the precision air valve, exhaust to atmospheric pressure, and control the exhaust time to 3min~5h; d. Control the first heating device to maintain the annealing temperature for annealing.

2. The method according to claim 1, characterized in that Also included is an air source device that can be selectively connected to the atmosphere communication conduit.

3. The method according to claim 1, characterized in that: The gas supply container is provided with a containing area for containing gas generating materials, the device also includes a second heating device for heating the containing area, and the connecting pipe is also provided with a pipeline temperature control device.

4. The method according to claim 1, characterized in that: The precision gas valve is a needle valve, a regulating valve, a diaphragm valve or a ball valve; And / or, an air outlet conduit is provided at the exhaust port, and the precision air valve is provided on the air outlet conduit; And / or, the horizontal placement area is the bottom of the film formation control container; And / or, the first heating device is an oil bath heating pot, a water bath heating pot or a steel ball heating pot.

5. The method according to claim 1, characterized in that The large-area perovskite polycrystalline film is covered on the bottom transmission layer, and the bottom transmission layer is combined on the transparent conductive substrate. In step a, the three-layer structure consisting of the large-area perovskite polycrystalline film, the bottom transmission layer and the transparent conductive substrate is placed in the horizontal placement area of ​​the film formation control container; the bottom transmission layer is an electron transmission layer or a hole transmission layer; And / or, the preset film forming temperature is 60°C to 250°C; And / or, the preset film forming pressure is 0.01-0.50 MPa; And / or, the annealing temperature is 70°C to 250°C, and the annealing time is 10min to 60min; and / or, before closing the precision gas valve, replacing the gas in the film formation control container and the gas supply container to ensure that the connected system formed by the film formation control container and the gas supply container is an inert atmosphere; And / or, the reaction gas is amine gas, alcohol gas or water vapor.

6. The method according to claim 1, characterized in that In step b, the reaction gas is continuously input into the film formation control container through the gas supply container until the preset film formation pressure is achieved: a gas generating material capable of generating reaction gas is added into the gas supply container, the gas generating material in the gas supply container is heated, and the reaction gas overflows into the film formation control container through the connecting pipe.

7. The method according to claim 1, characterized in that The step also includes: e. taking out the large-area perovskite single crystal film obtained after annealing and cooling it naturally at room temperature.

8. A method for preparing a solar cell, characterized in that: It includes: The large-area perovskite single crystal film prepared by the method according to any one of claims 1 to 7 is subjected to interface post-processing optimization, and then a top transport layer is prepared on the optimized large-area perovskite single crystal film, and then a top electrode is prepared on the top transport layer.

9. A solar cell, characterized in that: It is prepared by the preparation method of the solar cell according to claim 8, and the photoelectric conversion efficiency of the solar cell is greater than 20%.