A sandwich structured hollow fiber membrane with lining, and its preparation method and application
By adopting a sandwich structure design in the hollow fiber membrane and utilizing the interlocking structure of the polyvinylidene fluoride layer and the braided lining layer, the problems of insufficient mechanical strength and poor interface bonding force of traditional hollow fiber membranes are solved, achieving longer service life. lifespan and more stable operating performance.
Patent Information
- Application Number
- CN202410199464.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-23
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-23
AI Technical Summary
Traditional hollow fiber membranes have low mechanical strength and are prone to breakage under high-intensity air and water backwashing, resulting in a shortened service life of the membrane module. Moreover, the material difference between the braided liner and the membrane selective skin results in insufficient interface bonding force and prone to skin peeling. .
It adopts a sandwich structure lined hollow fiber membrane design. The cross-section of the membrane filament presents the structure of "polyvinylidene fluoride layer - braided lining layer - polyvinylidene fluoride layer" from the outside to the inside. Through the outer layer of the hydrophobic braided lining tube After coating the casting liquid, the inner and outer polyvinylidene fluoride layers penetrate into the gaps of the liner fabric and penetrate each other to improve the interface bonding strength.
It effectively improves the bonding strength between the polyvinylidene fluoride skin layer and the woven lining, avoids the shedding of the skin layer, extends the service life of the hollow fiber membrane, and maintains stable operation in the treatment of high turbidity and highly polluted wastewater.
Smart Images

Figure CN117797661B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hollow fiber membranes, and in particular to a sandwich-structured liner-type hollow fiber membrane and a preparation method and application thereof. Background Art
[0002] Membrane bioreactors have the characteristics of high separation efficiency, good effluent quality, low sludge production, impact resistance, and compact structure, and are widely used in the field of sewage and wastewater treatment. Hollow fiber membranes have high packing density and large specific surface area, and are widely used in membrane bioreactors. In order to effectively control the development of membrane fouling during operation and maintain the stable operation of the system, hollow fiber membrane components require frequent online air-water backwashing. Traditional hollow fiber membrane components have low mechanical strength and are prone to wire breakage under high-intensity air-water backwashing, which greatly reduces the service life of the membrane components. Introducing a braided liner support layer into the hollow fiber membrane, that is, preparing a lined hollow fiber membrane, is an effective means to improve the mechanical strength of the membrane fiber and ensure the stable operation of the membrane bioreactor system.
[0003] The braided liner as a support layer is usually made of a different material from the membrane's selective cortex, resulting in weak interface bonding. The cortex is prone to shedding during use, so it is particularly important to improve the bonding strength between the cortex and the liner. CN102160967A discloses a method for improving the interface bonding strength of a liner-enhanced hollow fiber membrane tube by secondary coating. Compared with the casting liquid, hydrophobic nanopowder is added to the pre-coating transition layer blending stock solution, which improves the adhesion and hardness of the transition layer and its compatibility with the surface separation layer. The volume shrinkage rate during the phase inversion process is extremely small, and the interface stability is improved. CN106268361A discloses a process for pretreating the liner. The pretreatment liquid used is one of the solvent, non-solvent or solvent / non-solvent mixture of the polymer raw material of the casting liquid. After the liner is immersed in the pretreatment liquid for a period of time, the excess pretreatment liquid is removed, and the liner is restored to a round shape and used for spinning. This process can effectively improve the bonding strength between the cortex and the liner and avoid cortex peeling. Zhu Mingxing et al. proposed a method for surface modification of braided liner using silane coupling agent KH-550. This method improves the surface roughness and specific surface area of the braided liner, promotes the wetting process of the casting liquid on the braided liner, strengthens the mechanical meshing and physical adsorption bonding between the casting liquid and the liner, and greatly improves the interfacial bonding strength of the composite membrane. However, the problem of material compatibility cannot be fundamentally solved by treating the surface of the braided liner alone, and the stability between the separation layer and the liner still needs to be improved. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a sandwich-structured lined hollow fiber membrane and a preparation method and application thereof. The present invention only requires coating the casting liquid on the outer layer of the hydrophobic braided lining tube. The membrane fiber cross-section of the prepared hollow fiber membrane presents a sandwich structure of "polyvinylidene fluoride layer-braided lining layer-polyvinylidene fluoride layer" from the outside to the inside. The inner and outer polyvinylidene fluoride layers penetrate each other by infiltrating the gaps in the liner tube fabric, effectively improving the bonding strength between the outer polyvinylidene fluoride skin layer and the braided lining.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a sandwich structured hollow fiber membrane with a liner, comprising the following steps:
[0007] The polyvinylidene fluoride, solvent, additive and porogen are heated, mixed and degassed to obtain a casting solution; the mass concentration of the polyvinylidene fluoride in the casting solution is 10-20%;
[0008] Performing hydrophobic modification on the braided inner liner to obtain a hydrophobic braided inner liner;
[0009] The casting solution and the hydrophobic braided inner liner are subjected to coaxial spinning, air bath and coagulation bath in sequence to obtain membrane filaments; during the coaxial spinning, the hydrophobic braided inner liner passes through the inner layer of the double-layer spinneret, and the casting solution passes through the outer layer of the double-layer spinneret;
[0010] The membrane fibers are sequentially immersed in water and immersed in glycerol, and dried to obtain a sandwich-structured hollow fiber membrane with a liner.
[0011] Preferably, the material of the braided lining layer includes polyethylene terephthalate.
[0012] Preferably, the additives in the casting solution include macromolecular additives and / or small molecule additives, wherein the macromolecular additives include polyvinyl pyrrolidone and / or polyvinyl alcohol; and the small molecule additives include ethanol and / or glycerol.
[0013] Preferably, the casting solution comprises the following components in percentage by weight:
[0014] Polyvinylidene fluoride 10~20%;
[0015] Macromolecular additives 3~10%;
[0016] Small molecule additives 0~3%;
[0017] Porogen 3~10%;
[0018] Solvent 60~84%.
[0019] Preferably, the hydrophobic modification method comprises the following steps:
[0020] The braided liner tube is sequentially cleaned with a NaOH solution and treated with a low-temperature plasma; the atmosphere of the low-temperature plasma treatment includes argon and carbon tetrafluoride.
[0021] Preferably, during the coaxial spinning, the temperature of the casting solution is 60-85°C;
[0022] The roller traction speed is 5~50 m / min;
[0023] The air gap of the air bath is 0.5 to 30 cm;
[0024] The liquid of the coagulation bath is water, the temperature of the coagulation bath is 30-70°C, and the time is 2-30 s.
[0025] Preferably, the time for the water immersion treatment is 12 to 48 hours, and the time for the glycerol immersion treatment is 12 to 48 hours.
[0026] The present invention provides a sandwich structured liner-type hollow fiber membrane prepared by the above preparation method, wherein the membrane layers of the hollow fiber membrane sequentially include an inner polyvinylidene fluoride layer, a woven inner liner layer and an outer polyvinylidene fluoride layer from inside to outside.
[0027] Preferably, the thickness of the inner polyvinylidene fluoride layer is 100-200 μm, the thickness of the braided lining layer is 200-1000 μm, and the thickness of the outer polyvinylidene fluoride layer is 100-200 μm;
[0028] The inner diameter of the membrane fibers of the hollow fiber membrane is 0.7-1.9 mm.
[0029] The present invention provides the use of the sandwich structured liner-type hollow fiber membrane in a membrane bioreactor.
[0030] The invention provides a method for preparing a sandwich-structured hollow fiber membrane with a lining, comprising the following steps: heating and mixing polyvinylidene fluoride, a solvent, an additive and a porogen and degassing to obtain a casting solution; the mass concentration of polyvinylidene fluoride in the casting solution is 10-20%; hydrophobically modifying a braided lining tube to obtain a hydrophobic braided lining tube; sequentially subjecting the casting solution and the hydrophobic braided lining tube to coaxial spinning, air bathing and coagulation bathing to obtain membrane filaments; during the coaxial spinning, the hydrophobic braided lining tube passes through the inner layer of a double-layer spinneret, and the casting solution passes through the outer layer of the double-layer spinneret; sequentially subjecting the membrane filaments to water immersion treatment and glycerol immersion treatment, and drying to obtain a sandwich-structured hollow fiber membrane with a lining. The present invention achieves the effect of reducing the viscosity of the casting liquid by controlling the mass concentration of polyvinylidene fluoride in the casting liquid to 10-20%; the present invention can improve the solvent wettability of the braided liner by performing hydrophobic modification on the braided liner; the present invention only needs to coat the casting liquid on the outer layer of the hydrophobic braided liner, and the operation is simple. By means of reducing the viscosity of the casting liquid, improving the solvent wettability of the braided liner, and prolonging the infiltration time, the casting liquid coated on the outer layer of the braided liner can fully infiltrate and penetrate the braided fiber, and a phase separation process occurs on both the inside and outside of the liner to obtain a lined hollow fiber membrane with a "polyvinylidene fluoride layer-braided liner layer-polyvinylidene fluoride layer" sandwich structure. The inner and outer polyvinylidene fluoride layers penetrate each other by infiltrating into the gaps of the liner fabric to form an interlocking structure, thereby improving the bonding strength between the polyvinylidene fluoride cortex and the braided liner and preventing the cortex from falling off.
[0031] At the same time, the preparation method provided by the present invention is simple to operate, low in cost, and easy to realize industrial mass production.
[0032] The present invention only requires coating the casting liquid on the outer layer of the hydrophobic braided liner tube, and the membrane fibers in the prepared sandwich-structured lined hollow fiber membrane have a sandwich structure of "polyvinylidene fluoride layer-braided liner layer-polyvinylidene fluoride layer". The inner and outer polyvinylidene fluoride layers penetrate each other by infiltrating the gaps in the liner tube fabric, effectively improving the bonding strength between the outer polyvinylidene fluoride cortex and the braided liner, avoiding the shedding of the cortex, and extending the service life and application range of the hollow fiber membrane. This interlocking structure can overcome the problem of unstable structure between the separation layer and the lining layer in the "separation layer-lining layer" structure of the traditional lined hollow fiber membrane, and easy peeling during frequent backwashing, improve the stability of the membrane structure, and can be operated in both internal pressure and external pressure forms. The sandwich-structured lined hollow fiber membrane provided by the present invention can withstand high-intensity online water-gas backwashing operations in membrane bioreactors, and is suitable for the treatment of high-turbidity, highly polluted wastewater and high-biomass membrane bioreactors. The results of the embodiments show that the sandwich-structured lined hollow fiber membrane provided by the present invention treats domestic sewage in the form of MBR, and the membrane flux is 10-15 LMH under stable operation at 50 KPa, and the effluent turbidity is less than 1 NTU. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a cross-sectional schematic diagram of a sandwich structured hollow fiber membrane with a liner according to the present invention;
[0034] Figure 2 This is a cross-sectional electron microscope photograph of the sandwich structured hollow fiber membrane with liner obtained in Example 1;
[0035] Figure 3 This is a cross-sectional electron microscope photograph of the lined hollow fiber membrane obtained in Comparative Example 1. DETAILED DESCRIPTION
[0036] The present invention provides a method for preparing a sandwich structured hollow fiber membrane with a liner, comprising the following steps:
[0037] The polyvinylidene fluoride, solvent, additive and porogen are heated, mixed and degassed to obtain a casting solution; the mass concentration of the polyvinylidene fluoride in the casting solution is 10-20%;
[0038] Performing hydrophobic modification on the braided inner liner to obtain a hydrophobic braided inner liner;
[0039] The casting solution and the hydrophobic braided inner liner are subjected to coaxial spinning, air bath and coagulation bath in sequence to obtain membrane filaments; during the coaxial spinning, the hydrophobic braided inner liner passes through the inner layer of the double-layer spinneret, and the casting solution passes through the outer layer of the double-layer spinneret;
[0040] The membrane fibers are sequentially immersed in water and immersed in glycerol, and dried to obtain a sandwich-structured hollow fiber membrane with a liner.
[0041] The present invention heats, mixes and degasses polyvinylidene fluoride, solvent, additive and porogen to obtain a casting solution. In the present invention, the additive in the casting solution preferably includes a macromolecular additive and / or a small molecule additive, and the macromolecular additive preferably includes polyvinyl pyrrolidone and / or polyvinyl alcohol, and the weight average molecular weight of the polyvinyl pyrrolidone is preferably 10K~360K, more preferably 50K~300K, and further preferably 100K~200K; the weight average molecular weight of the polyvinyl alcohol is preferably 25K~300K, more preferably 50K~200K, and further preferably 100K~150K.
[0042] In the present invention, the small molecule additive preferably includes ethanol and / or glycerol.
[0043] In the present invention, the casting solution preferably includes the following components in percentage by mass:
[0044] Polyvinylidene fluoride 10~20%;
[0045] Macromolecular additives 3~10%;
[0046] Small molecule additives 0~3%;
[0047] Porogen 3~10%;
[0048] Solvent 60~84%.
[0049] In terms of mass percentage, the casting solution includes 10-20% polyvinylidene fluoride, preferably 12-18%, and more preferably 15%. In the present invention, the molecular weight of the polyvinylidene fluoride is preferably 100K-650K, more preferably 200K-400K, and further preferably 300K.
[0050] In terms of mass percentage, the casting solution includes 3-10% of the macromolecular additive, preferably 5-8%.
[0051] In terms of mass percentage, the casting solution includes 0-3% of small molecule additives, preferably 1-2%.
[0052] In terms of mass percentage, the casting solution includes 3-10% of a porogen, preferably 5-8%. In the present invention, the porogen is preferably polyethylene glycol and / or polypropylene glycol, and the molecular weight of the porogen is preferably 200-6000, more preferably 500-5000, and further preferably 1000-3000.
[0053] In terms of mass percentage, the casting solution comprises 60-84% of solvent, preferably 70-80%. In the present invention, the solvent is preferably an organic solvent, more preferably one or more of N,N-dimethylacetamide, N,N-dimethylformamide and dimethyl sulfoxide.
[0054] The present invention achieves the effect of reducing the viscosity of the casting liquid by controlling the mass concentration of polyvinylidene fluoride in the casting liquid to 10-20% and the mass concentration of the macromolecular additive to 3-10%.
[0055] In the present invention, the temperature of the heating and mixing is preferably 60-85°C, more preferably 70-80°C; the time is preferably 12-24 h, more preferably 15-20 h; in the present invention, the heating and mixing is preferably stirring and mixing.
[0056] In the present invention, the degassing time is preferably 12 to 24 hours, more preferably 15 to 20 hours.
[0057] The present invention performs hydrophobic modification on a braided inner liner to obtain a hydrophobic braided inner liner. In the present invention, the material of the braided inner liner is preferably polyethylene terephthalate, the wall thickness of the braided inner liner is preferably 200-1000 μm, more preferably 500-800 μm, and the outer diameter is preferably 1-3 mm, more preferably 2 mm.
[0058] In the present invention, the method for hydrophobic modification preferably comprises the following steps:
[0059] The braided liner tube is sequentially cleaned with a NaOH solution and treated with a low-temperature plasma.
[0060] In the present invention, the mass concentration of the NaOH solution is preferably 3-7%, more preferably 5%, and the cleaning time of the NaOH solution is preferably 0.5-2 h. The present invention can effectively remove the oil stains on the braided inner liner tube by cleaning with the NaOH solution, and slightly corrode the surface of the braided inner liner tube to increase the roughness.
[0061] In the present invention, the atmosphere of the low temperature plasma treatment preferably includes argon and carbon tetrafluoride. In the present invention, the volume ratio of argon to carbon tetrafluoride is preferably 1:2 to 2:1, more preferably 2:1.
[0062] In the present invention, the power of the low-temperature plasma treatment is preferably 30-100 W, more preferably 50 W, and the time is preferably 30-600 s, more preferably 60 s. The present invention can introduce fluorine-containing functional groups on the surface of the braided liner fiber through the low-temperature plasma treatment to improve the hydrophobicity of the liner.
[0063] After obtaining the casting solution and the hydrophobic braided inner liner, the present invention sequentially performs coaxial spinning, air bath and coagulation bath on the casting solution and the hydrophobic braided inner liner to obtain membrane filaments; during the coaxial spinning, the hydrophobic braided inner liner passes through the inner layer of the double-layer spinneret, and the casting solution passes through the outer layer of the double-layer spinneret. In the present invention, the inner radius of the outer layer of the double-layer spinneret used for coaxial spinning is preferably 1.1-3.2 mm, more preferably 1.5-2.5 mm; the inner radius of the inner layer is preferably 0.7-1.9 mm, more preferably 1-1.5 mm.
[0064] In the present invention, during the coaxial spinning, the temperature of the casting solution is preferably 60-85°C; more preferably 70-80°C; the roller pulling speed is preferably 5-50 m / min, more preferably 10-30 m / min. The present invention controls the roller pulling speed at a relatively low rate of 5-50 m / min to achieve the effect of extending the infiltration time of the casting solution in the air bath.
[0065] In the present invention, the air gap of the air bath is preferably 0.5-30 cm, more preferably 5-20 cm; the liquid of the coagulation bath is water, the temperature of the coagulation bath is preferably 30-70 ° C, more preferably 40-60 ° C; the time is preferably 2-30 s, more preferably 10-20 s. The present invention can ensure that the casting liquid penetrates from the outer surface of the braided liner to the inner surface through the above-mentioned coaxial spinning, and completes the phase conversion process, thereby forming an inner polyvinylidene fluoride layer and an outer polyvinylidene fluoride layer.
[0066] After obtaining the membrane filaments, the present invention sequentially performs water immersion treatment and glycerol immersion treatment on the membrane filaments, and obtains a sandwich structured hollow fiber membrane with a liner after drying.
[0067] In the present invention, the time of the water immersion treatment is preferably 12 to 48 hours, more preferably 24 to 36 hours; the time of the glycerol immersion treatment is preferably 12 to 48 hours, more preferably 24 to 36 hours. The present invention can further remove solvents and additives through the water immersion treatment; the present invention can maintain the hydrophilicity of the membrane through the glycerol immersion treatment.
[0068] In the present invention, the drying method is preferably natural drying.
[0069] The present invention provides a sandwich structured liner-type hollow fiber membrane prepared by the above preparation method, wherein the membrane layers of the hollow fiber membrane sequentially include an inner polyvinylidene fluoride layer, a woven inner liner layer and an outer polyvinylidene fluoride layer from inside to outside.
[0070] In the present invention, the membrane fibers in the sandwich-structured hollow fiber membrane with lining have a sandwich structure of "polyvinylidene fluoride layer-woven inner lining layer-polyvinylidene fluoride layer", and the inner and outer polyvinylidene fluoride layers penetrate each other by penetrating into the gaps of the liner fabric.
[0071] In the present invention, the thickness of the inner polyvinylidene fluoride layer is preferably 100 to 200 μm, more preferably 120 to 180 μm, and further preferably 150 μm.
[0072] In the present invention, the material of the braided lining layer is preferably polyethylene terephthalate, and the thickness is preferably 200-1000 μm, more preferably 400-800 μm, and further preferably 500-600 μm.
[0073] In the present invention, the thickness of the outer polyvinylidene fluoride layer is preferably 100-200 μm, more preferably 120-180 μm, and further preferably 150 μm.
[0074] In the present invention, the inner diameter of the membrane fibers of the hollow fiber membrane is preferably 0.7 to 1.9 mm, more preferably 1 to 1.5 mm.
[0075] In the present invention, the effective membrane pore size of the sandwich-structured liner-type hollow fiber membrane is preferably 0.01 to 1 μm, more preferably 0.05 to 0.8 μm, and further preferably 0.1 to 0.5 μm.
[0076] In the present invention, the cross-sectional schematic diagram of the sandwich structured hollow fiber membrane with lining is as follows: Figure 1 shown. Figure 1 Among them, 1-outer polyvinylidene fluoride layer, 2-woven lining layer, 3-inner polyvinylidene fluoride layer.
[0077] The present invention provides the use of the sandwich structured hollow fiber membrane in a membrane bioreactor. In the present invention, the membrane bioreactor is preferably used for sewage and wastewater treatment.
[0078] The sandwich structured hollow fiber membrane with lining provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0079] Example 1
[0080] Weigh 42 g of polyvinylidene fluoride with an average molecular weight of 350K, 180 g of N,N-dimethylacetamide, 20 g of polyvinyl pyrrolidone with an average molecular weight of 40K, 5 g of propylene glycol, and 13 g of polyethylene glycol with a molecular weight of 6000, stir thoroughly at 70 °C for 12 h, and degas for 24 h to obtain a casting solution.
[0081] A 2.5 mm diameter, 300 μm wall-thick polyethylene terephthalate braided liner was used. The liner was cleaned with a 5 wt.% NaOH solution, dried, and placed in a low-temperature plasma device with an argon / carbon tetrafluoride volume ratio of 2:1, a power of 50 W, and a treatment time of 60 s.
[0082] The pretreated liner was installed on the spinning machine and passed through the center of the spinneret coaxially and vertically. The casting solution was kept at 70 °C, the pulling speed of the liner was 15 m / min, the air gap was 30 cm, the coagulation bath was water, the temperature was 50 °C, and the coagulation bath time was 10 s. The coagulated membrane was rinsed in 30 °C water for 12 h, immersed in glycerol solution for 12 h, and dried to obtain a sandwich structured hollow fiber membrane with liner.
[0083] The cross-sectional electron micrograph of the obtained sandwich structured hollow fiber membrane with lining is shown in FIG. Figure 2 As shown. Figure 2 It can be seen that the inner and outer PVDF layers penetrate each other by penetrating into the gaps of the liner fabric to form an interlocking structure.
[0084] Example 2
[0085] Weigh 31 g of polyvinylidene fluoride with an average molecular weight of 350K, 187 g of N,N-dimethylacetamide, 10 g of polyvinyl pyrrolidone with an average molecular weight of 30K, 7 g of propylene glycol, and 25 g of polyethylene glycol with a molecular weight of 6000, stir thoroughly for 12 h at 70 °C, and degas for 24 h to obtain a casting solution. The liner modification and membrane preparation process are the same as in Example 1. The cross section of the obtained lined hollow fiber membrane presents a sandwich structure of "polyvinylidene fluoride layer-woven liner layer-polyvinylidene fluoride layer".
[0086] Example 3
[0087] Weigh 49 g of polyvinylidene fluoride with an average molecular weight of 650K, 159 g of N,N-dimethylacetamide, 26 g of polyvinyl pyrrolidone with an average molecular weight of 30K, 6 g of propylene glycol, and 20 g of polyethylene glycol with a molecular weight of 2000, stir them thoroughly at 70 °C for 12 h, and degas for 24 h to obtain a casting solution. The liner modification and membrane preparation process are the same as in Example 1. The cross section of the obtained lined hollow fiber membrane presents a sandwich structure of "polyvinylidene fluoride layer-woven liner layer-polyvinylidene fluoride layer".
[0088] Comparative Example 1
[0089] Weigh 49 g of polyvinylidene fluoride with an average molecular weight of 650K, 159 g of N,N-dimethylacetamide, 26 g of polyvinyl pyrrolidone with an average molecular weight of 30K, 6 g of propylene glycol, and 20 g of polyethylene glycol with a molecular weight of 2000, stir thoroughly at 70 °C for 12 h, and degas for 24 h to obtain a casting solution.
[0090] A 2.5 mm diameter, 300 μm wall thickness polyethylene terephthalate braided liner was used, and the liner was cleaned with a 5wt.% NaOH solution. The cleaned liner was installed on the spinning machine and passed coaxially and vertically through the center of the spinneret. The casting solution was kept at 70 °C, the liner pulling speed was 15 m / min, the air gap was 30 cm, the coagulation bath was water, the temperature was 50 °C, and the coagulation bath time was 10 s. The coagulated membrane was rinsed in 30 °C water for 12 h, immersed in a glycerol solution for 12 h, and dried. No endothelial layer was observed in the cross section of the obtained lined hollow fiber membrane.
[0091] The cross-sectional electron micrograph of the obtained hollow fiber membrane with lining is shown in FIG. Figure 3 It can be seen that the obtained lining type hollow fiber membrane does not have a sandwich structure of "polyvinylidene fluoride layer-woven lining layer-polyvinylidene fluoride layer".
[0092] Comparative Example 2
[0093] Weigh 55 g of polyvinylidene fluoride with an average molecular weight of 650K, 140 g of N,N-dimethylacetamide, 39 g of polyvinyl pyrrolidone with an average molecular weight of 58K, 6 g of propylene glycol, and 20 g of polyethylene glycol with a molecular weight of 2000, stir thoroughly at 70 °C for 12 h, and degas for 24 h to obtain a casting solution.
[0094] The modification of the liner is the same as in Example 1. The liner is installed on the spinning machine and passed coaxially and vertically from the center of the spinneret. The casting solution is kept at 70 °C, the pulling speed of the liner is 15 m / min, the air gap is 30 cm, the coagulation bath is water, the temperature is 50 °C, and the coagulation bath time is 10 s. The coagulated membrane is rinsed in 30 °C water for 12 h, immersed in a glycerol solution for 12 h, and dried. No endothelial layer is observed in the cross section of the obtained hollow fiber membrane with liner.
[0095] Comparative Example 3
[0096] Weigh 49 g of polyvinylidene fluoride with an average molecular weight of 650K, 159 g of N,N-dimethylacetamide, 26 g of polyvinyl pyrrolidone with an average molecular weight of 30K, 6 g of propylene glycol, and 20 g of polyethylene glycol with a molecular weight of 2000, stir thoroughly at 70 °C for 12 h, and degas for 24 h to obtain a casting solution.
[0097] The modification of the liner is the same as in Example 1. The liner is installed on the spinning machine and passed coaxially and vertically from the center of the spinneret. The casting solution is kept at 70 °C, the pulling speed of the liner is 60 m / min, the air gap is 10 cm, the coagulation bath is water, the temperature is 50 °C, and the coagulation bath time is 10 s. The coagulated membrane is rinsed in 30 °C water for 12 h, immersed in a glycerol solution for 12 h, and dried. No endothelial layer is observed in the cross section of the obtained hollow fiber membrane with liner.
[0098] Performance Testing
[0099] ①Cortex peel strength test method:
[0100] The isomorphic internal pressure method is used to test the bonding strength between the braided tube and the cortex. The method is as follows: a 15 cm membrane fiber sample is cast into a dead-end filtration membrane assembly. An internal pressure backwash operation is performed with pure water as the medium at 0.1 MPa for 2 h. Thereafter, the internal pressure is gradually increased by 0.02 MPa each time and maintained for 0.5 h. The pressure when the surface separation layer is damaged is the peel strength of the membrane fiber.
[0101] According to the test, compared with the hollow fiber membrane obtained in comparative example 1, the peeling strength of the skin layer of the mesoporous fiber membrane with a sandwich structure in Examples 1, 2 and 3 can be increased by 56%, 11% and 50%, respectively.
[0102] ②Water treatment test:
[0103] The lined hollow fiber membrane in Example 1 was used to treat domestic sewage in the form of MBR, with an initial turbidity of 30-40 NTU, a membrane flux of 15 LMH under stable operation at 50 kPa, and an effluent turbidity of less than 1 NTU.
[0104] The lined hollow fiber membrane in Example 2 was used to treat domestic sewage in the form of MBR. The membrane flux was measured to be 12 LMH under stable operation at 50 kPa, and the effluent turbidity was less than 1 NTU.
[0105] The lined hollow fiber membrane in Example 3 was used to treat domestic sewage in the form of MBR. The membrane flux was measured to be 10 LMH under stable operation at 50 kPa, and the effluent turbidity was less than 1 NTU.
[0106] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a sandwich structured hollow fiber membrane with a liner, comprising the following steps: The polyvinylidene fluoride, solvent, additive and porogen are heated, mixed and degassed to obtain a film casting solution; The braided inner liner tube is hydrophobically modified to obtain a hydrophobic braided inner liner tube; the braided inner liner tube is made of polyethylene terephthalate, has a wall thickness of 300 μm, and a diameter of 2.5 mm; The casting solution and the hydrophobic braided inner liner are subjected to coaxial spinning, air bath and coagulation bath in sequence to obtain membrane filaments; during the coaxial spinning, the hydrophobic braided inner liner passes through the inner layer of the double-layer spinneret, and the casting solution passes through the outer layer of the double-layer spinneret; The membrane fibers are sequentially immersed in water and immersed in glycerol, and dried to obtain a sandwich-structured hollow fiber membrane with a liner; The additive in the casting solution is a macromolecular additive and / or a small molecule additive, wherein the macromolecular additive is polyvinyl pyrrolidone and / or polyvinyl alcohol; the small molecule additive is ethanol and / or glycerol; and the solvent is an organic solvent; The casting solution is composed of the following components in percentage by weight: Polyvinylidene fluoride 10~20%; Macromolecular additives 3~10%; Small molecule additives 1~3%; Porogen 3~10%; Solvent 60~84%; The method for hydrophobic modification comprises the following steps: The braided liner tube is sequentially cleaned with a NaOH solution and treated with a low-temperature plasma; the mass concentration of the NaOH solution is 3-7%; the atmosphere of the low-temperature plasma treatment includes argon and carbon tetrafluoride; the volume ratio of argon to carbon tetrafluoride is 1:2-2:1; The power of the low-temperature plasma treatment is 30-100 W, and the time is 30-600 s; During the coaxial spinning, the temperature of the casting solution is 60-85°C; The roller traction speed is 5~50 m / min; The air gap of the air bath is 0.5 to 30 cm; The liquid of the coagulation bath is water, the temperature of the coagulation bath is 30-70°C, and the time is 2-30 s; The time of the water immersion treatment is 12 to 48 hours, and the time of the glycerol immersion treatment is 12 to 48 hours.
2. The sandwich-structured lined hollow fiber membrane prepared by the preparation method of claim 1, wherein the membrane layers of the hollow fiber membrane include, from inside to outside, an inner polyvinylidene fluoride layer, a woven inner lining layer and an outer polyvinylidene fluoride layer.
3. The sandwich structured hollow fiber membrane with lining according to claim 2, characterized in that: The thickness of the inner polyvinylidene fluoride layer is 100-200 μm, the thickness of the braided lining layer is 200-1000 μm, and the thickness of the outer polyvinylidene fluoride layer is 100-200 μm; The inner diameter of the membrane fibers of the hollow fiber membrane is 0.7-1.9 mm.
4. Use of the sandwich-structured lined hollow fiber membrane according to any one of claims 2 to 3 in a membrane bioreactor.