A dry and ultra-wear-resistant organic silicon leather surface treatment agent, and its preparation and application

By preparing a silicone leather surface treatment agent containing components such as vinyl silicone oil, vinyl fluorosilicon oil, etc., the problem of lack of suitable treatment agent for silicone leather in the prior art is solved, and the dry slippery and wear resistance of silicone leather is achieved Features, suitable for a variety of daily necessities.

CN117801675BActive Publication Date: 2024-11-12WUHAN INSTITUTES OF ADVANCED TECHNOLOGY CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311845472.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-11-12
Estimated Expiration
2043-12-28

AI Technical Summary

Technical Problem

Leather surface treatment agents on the existing market are not suitable for silicone leather, and there is a lack of effective silicone leather surface treatment agents.

Method used

Provides a dry, ultra-wear-resistant silicone leather surface treatment agent, including vinyl silicone oil, vinyl fluorosilicone oil, polyether modified silicone oil, wax powder, matting powder, catalyst and hydrogen-containing silicone oil, through specific ratios and stirring steps Prepare to form a surface treatment agent suitable for silicone leather.

Benefits of technology

It significantly improves the wear resistance of silicone leather, making its surface dry slippery and wear-resistant, fills the gap in the silicone leather surface treatment agent market, provides a new solution, and is simple in the formulation and raw material Easy to find, suitable for household textiles, clothing daily necessities and automotive interiors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117801675B_ABST
    Figure CN117801675B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of silicone leather, and more specifically, relates to a dry and super wear-resistant silicone leather surface treatment agent, and its preparation and application. The dry and super wear-resistant silicone surface treatment agent provided by the present invention significantly improves the wear resistance of silicone leather by compounding components such as vinyl silicone oil, vinyl fluorosilicone oil and polyether modified silicone oil, especially the introduction of vinyl fluorosilicone oil, and obtains a dry and super wear-resistant silicone leather surface treatment agent that is particularly suitable for silicone leather. The silicone leather surface treatment agent of the present invention has a simple formula, and the formula raw materials are easy to obtain. It does not need to be designed and synthesized separately, and has the characteristics of wide repeatability. It enriches the existing types of leather treatment agents and fills the gap in the market of silicone leather surface treatment agents.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of organic silicon leather, and more specifically, relates to a dry and ultra-wear-resistant organic silicon leather surface treatment agent, and its preparation and application. Background Art

[0002] Currently, artificial leather is mostly made of polyurethane, PVC, PE and other types of leather, but their main disadvantage is poor aging performance; silicone leather is durable, soft, and has good tensile strength, but it feels astringent and needs to be treated on the surface. Applying silicone surface treatment agent on the leather surface can make the leather surface dry, smooth and wear-resistant.

[0003] The leather surface treatment agents sold on the market are mainly for polyurethane-type leather. The polyurethane molecular chains in the treatment agents are grafted with silicone molecules, which have high polarity and can migrate to the surface of polyurethane-type leather, thus having dry and slippery properties. The leather surface treatment agents currently sold on the market for polyurethane-type leather contain polydimethylsiloxane, which mainly plays a role in providing a smooth feeling. The silicone in silicone leather is mainly polydimethylsiloxane, and the two are of the same type of material. The polydimethylsiloxane contained in the leather surface treatment agents for polyurethane-type leather will not migrate to the surface of silicone leather, so the surface treatment agents on the market are not suitable for silicone leather. It is imperative to develop new surface treatment agents suitable for silicone leather. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a dry and ultra-wear-resistant silicone leather surface treatment agent, and its preparation and application, so as to solve the technical problems that the prior art surface treatment agents are not suitable for silicone leather and there is a lack of effective silicone leather surface treatment agents.

[0005] To achieve the above-mentioned purpose, the present invention provides a dry and super wear-resistant silicone leather surface treatment agent, characterized in that it comprises, by weight: 60-80 parts of vinyl silicone oil; 10-15 parts of vinyl fluorosilicone oil; 0.1-1 part of polyether modified silicone oil; 0.5-2 parts of wax powder; 10-15 parts of matting powder; 0.2-1 part of catalyst; 0.02-1 part of inhibitor; and 10-15 parts of hydrogen-containing silicone oil.

[0006] Preferably, the viscosity of the vinyl silicone oil is 20000-50000 Pa﹒s.

[0007] Preferably, the vinyl fluorosilicone oil contains 10 to 30% fluorine and 0.0143 to 0.0184 mol / 100g vinyl.

[0008] Preferably, the polyether-modified silicone oil is synthesized by inserting polyether and alkylene oxide into the chain segments of polymethylsiloxane macromolecules, and has a viscosity of 700-1000 Pa﹒s and an epoxy content of 1.55-1.9wt%.

[0009] Preferably, the wax powder is a modified PE wax powder having a melting point lower than 120°C.

[0010] Preferably, the particle size of the matting powder is between 1 and 15 μm, and more preferably between 2 and 10 μm.

[0011] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 0.79 to 1.55 mol / 100 g; the silicon-hydrogen ratio is between 1 and 1.2; and the hydrogen-containing silicone oil comprises side chain hydrogen-containing silicone oil and terminal chain hydrogen-containing silicone oil.

[0012] According to another aspect of the present invention, there is provided a method for preparing the surface treatment agent, comprising the following steps:

[0013] (1) adding the vinyl silicone oil, vinyl fluorinated silicone oil, polyether modified silicone oil and wax powder in sequence according to weight ratio and stirring evenly;

[0014] (2) adding the inhibitor, matting powder and hydrogenated silicone oil and stirring evenly;

[0015] (3) Finally, add the catalyst and stir evenly to obtain the surface treatment agent.

[0016] According to another aspect of the present invention, there is provided a use of the surface treatment agent as a silicone leather surface treatment agent.

[0017] In general, the above technical solution conceived by the present invention has the following advantages compared with the prior art:

[0018] Beneficial effects:

[0019] (1) The present invention provides a dry and super wear-resistant silicone surface treatment agent, which significantly improves the wear resistance of silicone leather by compounding components such as vinyl silicone oil, vinyl fluorosilicone oil and polyether modified silicone oil, especially the introduction of vinyl fluorosilicone oil, thereby obtaining a dry and super wear-resistant silicone leather surface treatment agent that is particularly suitable for silicone leather.

[0020] (2) The organic silicon leather surface treatment agent of the present invention has a simple formula, and the raw materials are easily available, and it does not need to be designed and synthesized separately, and it has the characteristics of wide repetitive operation. There are basically no surface treatment agents suitable for organic silicon coatings on the market. The present invention is the first implementable organic silicon surface treatment agent, which can make the surface of organic silicon leather have dry, smooth and wear-resistant properties after use, providing a new solution for organic silicon type leather treatment agents, enriching the existing types of leather treatment agents, and filling the gap in the organic silicon leather surface treatment agent market.

[0021] (3) The preparation method of the silicone leather surface treatment agent of the present invention is simple. The key is to evenly disperse the materials. When used, the surface treatment agent is coated and cured to form a dense treatment layer on the surface of the silicone leather, making the silicone leather dry and super wear-resistant. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 These are surface photographs of the silicone leather surface treatment agent according to the embodiment of the present invention and the control sample after curing and rubbing 10,000 times. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0024] The present invention provides a dry and super wear-resistant organic silicon leather surface treatment agent, which comprises, by weight, 60-80 parts of vinyl silicone oil, 10-15 parts of vinyl fluorosilicone oil, 0.1-1 part of polyether modified silicone oil, 0.5-2 parts of wax powder, 10-15 parts of matting powder, 0.2-1 part of catalyst, 0.02-1 part of inhibitor and 10-15 parts of hydrogen-containing silicone oil.

[0025] In order to improve the wear resistance of the surface treatment agent, in some embodiments of the present invention, the vinyl silicone oil is a high-viscosity vinyl silicone oil, for example, in some embodiments, the viscosity is 20,000-50,000 Pa﹒s, and preferably, terminal-chain vinyl silicone oil is selected, that is, the vinyl groups are located at both ends of the silicone oil.

[0026] The present invention introduces vinyl fluorosilicone oil into the formulation of the surface treatment agent. Experiments have found that the introduction of vinyl fluorosilicone oil can reduce its surface tension and improve its wear resistance. However, the fluorine content of the vinyl fluorosilicone oil should not be too high, otherwise the polarity is too large, the steric hindrance effect hinders polymerization, and it is difficult to form a cross-linked network. In some embodiments, the fluorine content in the vinyl fluorosilicone oil is 10-30%, and the vinyl content is 0.0143-0.0184 mol / 100g. In the embodiment, a vinyl fluorosilicone oil with a fluorine content of 30% and a vinyl content of 0.0143 mol / 100g is selected, and its structure is as follows:

[0027]

[0028] In some embodiments, the polyether-modified silicone oil is a polyether-epoxy co-modified silicone oil, which is synthesized by inserting polyether macromolecules and alkylene oxides into the chain segments of polymethylsiloxane macromolecules, and has a viscosity of 700-1000 Pa﹒s and an epoxy content of 1.55-1.9wt%. The polyether-modified silicone oil of the present invention is used to increase the leveling property of the surface treatment agent, and is generally added in an amount of 0.1-1 part in consideration of cost and material strength.

[0029] In some embodiments, the wax powder is a modified PE wax powder, whose melting point is generally below 120°C, and the curing temperature of the surface treatment agent is between 120 and 150°C. After high-temperature heating, the wax powder can facilitate the dispersion and leveling of the surface treatment agent and enhance the hand feel. The preferred addition amount is 0.5 to 2 parts.

[0030] In some embodiments, the particle size of the matting powder is between 1 and 15 μm, preferably between 2 and 10 μm. For colored materials, the matting powder is generally used for matting. In addition to the matting effect, the matting powder of the present invention has a certain influence on the wear resistance of the silicone leather surface treatment agent due to its different particle sizes. The surface treatment agent prepared by the matting powder with a larger particle size has relatively better wear resistance.

[0031] In some embodiments, the catalyst is a platinum catalyst, and the platinum catalyst includes but is not limited to one of the types such as chloroplatinic acid isopropanol solution, chloroplatinic acid tetrahydrofuran solution, chloroplatinic acid-divinyltetramethyldisiloxane complex, chloroplatinic acid-1,3,5,7-tetravinyl-1,3,5,7-tetramethyl-cyclotetrasiloxane, and chloroplatinic acid-divinyltetramethyldisiloxane. In a preferred embodiment, a chloroplatinic acid isopropanol solution with a platinum content of 5000 ppm is selected, and the amount added is 0.2 to 1 parts.

[0032] In some embodiments, the inhibitor is methylbutynol, and the amount added is 0.02 to 1 parts. The inhibitor is added mainly to regulate the reaction rate. It is generally added before the catalyst, that is, the catalyst is added after the inhibitor is added and dispersed. If the catalyst is added in advance, the part where the inhibitor is added is prone to react prematurely and form lumps.

[0033] In some embodiments, the hydrogen content of the hydrogen-containing silicone oil is 0.79-1.55 mol / 100 g. The hydrogen-containing silicone oil of the present invention is a cross-linking agent. Generally, the hydrogen-containing silicone oil of the end chain and the hydrogen-containing silicone oil of the side chain are compounded as needed (the end chain and the side chain contain Si-H bonds respectively) to achieve the purpose of chain extension and increase the cross-linking network density. The amount added is proportioned with the amount of vinyl silicone oil added, and the silicon-hydrogen ratio is selected between 1 and 1.2.

[0034] The present invention also provides a method for preparing the surface treatment agent, comprising the following steps:

[0035] (1) adding the vinyl silicone oil, vinyl fluorinated silicone oil, polyether modified silicone oil and wax powder in sequence according to weight ratio, and stirring to evenly disperse the wax powder therein;

[0036] (2) adding the inhibitor, matting powder and hydrogen-containing silicone oil, and stirring to disperse the matting powder;

[0037] (3) Finally, add the catalyst and stir evenly to obtain the surface treatment agent.

[0038] The surface treatment agent provided by the present invention can be used as a surface treatment agent for silicone leather. It relates to the field of silicone leather, and specifically to the first half of the treatment of silicone leather preparation, so that the surface of the silicone leather has dry, slippery and wear-resistant properties, and is widely used in household textiles, clothing daily necessities, automobile interiors, etc., to meet people's demand for high-quality daily necessities.

[0039] "Dayi" mentioned in some sources of raw materials used in the following examples refers to Shandong Dayi Chemical Co., Ltd., "Lingwei" refers to Guangzhou Lingwei Technology Co., Ltd., "Runhe" refers to Ningbo Runhe High-tech Materials Technology Co., Ltd., and "Tianshi" refers to Nanjing Tianshi New Materials Technology Co., Ltd.

[0040] Example 1

[0041] The dry and super wear-resistant organic silicon leather surface treatment agent of this embodiment includes, by weight, 75 parts of vinyl silicone oil (viscosity of 20000 Pa﹒s, vinyl content of 0.0514 mol / 100 g, Dayi DY-V401-20000), 10 parts of vinyl fluorosilicone oil (fluorine content of 30%, vinyl content of 0.0143 mol / 100 g, Xinyuan Chemical (Shandong) Co., Ltd., product brand NFS7300-G30), 0.5 parts of polyether epoxy co-modified silicone oil (Dayi DY-ETE301H), 1 part of wax powder (Tianshi Twax-1411), 10 parts of matting powder (Lingwei-10, average particle size of 10 μm), 0.5 parts of catalyst (5000 ppm chloroplatinic acid isopropanol solution), 0.02 parts of inhibitor methyl butynol, 13 parts of hydrogen-containing silicone oil (including Runhe RH-LHC-3 3 parts and Runhe RH-H6 10 parts). The preparation steps are as follows:

[0042] Step 1: First, add 75 parts of vinyl silicone oil, 10 parts of vinyl fluorine-containing silicone oil, 0.5 parts of polyether epoxy co-modified silicone oil, and 1 part of wax powder in sequence according to weight parts, stir evenly, and make the wax powder evenly dispersed therein;

[0043] Step 2: Add 0.02 parts of inhibitor, 10 parts of matting powder, and 13 parts of hydrogenated silicone oil, and stir evenly to disperse the matting powder;

[0044] Step 3: Finally, add 0.5 parts of catalyst and stir evenly to obtain the surface treatment agent.

[0045] Example 2

[0046] The dry and super wear-resistant organic silicon leather surface treatment agent of this embodiment includes 75 parts of vinyl silicone oil (viscosity of 20000 Pa﹒s, vinyl content of 0.0514 mol / 100g), 10 parts of vinyl fluorosilicone oil (fluorine content of 30%, vinyl content of 0.0143 mol / 100g, Xinyuan Chemical (Shandong) Co., Ltd., product brand NFS7300-G30), 0.5 parts of polyether epoxy co-modified silicone oil (Dayi DY-ETE301H), 1 part of wax powder (Tianshi Twax-1411), 10 parts of matting powder (Lingwei-2, average particle size of 2μm), 0.5 parts of catalyst (5000ppm chloroplatinic acid isopropanol solution), 0.02 parts of inhibitor methyl butynol, and 13 parts of hydrogen-containing silicone oil (including 3 parts of Runhe RH-LHC-3 and 10 parts of Runhe RH-H6). The preparation steps are as follows:

[0047] Step 1: First, add 75 parts of vinyl silicone oil, 10 parts of vinyl fluorine-containing silicone oil, 0.5 parts of polyether epoxy co-modified silicone oil, and 1 part of wax powder in sequence according to weight parts, stir evenly, and make the wax powder evenly dispersed therein;

[0048] Step 2: Add 0.02 parts of inhibitor, 10 parts of matting powder, and 13 parts of hydrogenated silicone oil, and stir evenly to disperse the matting powder;

[0049] Step 3: Finally, add 0.5 parts of catalyst and stir evenly to obtain the surface treatment agent.

[0050] Comparative Example 1

[0051] The dry and super wear-resistant organic silicon leather surface treatment agent of this embodiment includes 75 parts of vinyl silicone oil (viscosity of 20000 Pa﹒s, vinyl content of 0.0514 mol / 100g), 0.5 parts of polyether epoxy co-modified silicone oil (Dayi DY-ETE301H), 1 part of wax powder, 10 parts of matting powder (Lingwei-10, average particle size of 10μm), 0.5 parts of catalyst (5000ppm chloroplatinic acid isopropanol solution), 0.02 parts of inhibitor, and 13 parts of hydrogen-containing silicone oil (including 3 parts of Runhe RH-LHC-3 and 10 parts of Runhe RH-H6) by weight. The preparation steps are as follows:

[0052] Step 1: First, add 75 parts of vinyl silicone oil, 10 parts of vinyl fluorine-containing silicone oil, 0.5 parts of polyether epoxy co-modified silicone oil, and 1 part of wax powder in sequence according to weight parts, stir evenly, and make the wax powder evenly dispersed therein;

[0053] Step 2: Add 0.02 parts of inhibitor, 10 parts of matting powder, and 13 parts of hydrogenated silicone oil, and stir evenly to disperse the matting powder;

[0054] Step 3: Finally, add 0.5 parts of catalyst and stir evenly to obtain the surface treatment agent.

[0055] Comparative Example 2

[0056] The dry and super wear-resistant organic silicon leather surface treatment agent of this embodiment includes, by weight, 75 parts of vinyl silicone oil (viscosity of 20000 Pa﹒s, vinyl content of 0.0514 mol / 100g), 0.5 parts of polyether epoxy co-modified silicone oil (Dayi DY-ETE301H), 1 part of wax powder (Tianshi Twax-1411), 10 parts of matting powder (Lingwei-2, average particle size of 2μm), 0.5 parts of catalyst (5000ppm chloroplatinic acid isopropanol solution), 0.02 parts of inhibitor methyl butynol, and 13 parts of hydrogen-containing silicone oil (including 3 parts of Runhe RH-LHC-3 and 10 parts of Runhe RH-H6). The preparation steps are as follows:

[0057] Step 1: First, add 75 parts of vinyl silicone oil, 10 parts of vinyl fluorine-containing silicone oil, 0.5 parts of polyether epoxy co-modified silicone oil, and 1 part of wax powder in sequence according to weight parts, stir evenly, and make the wax powder evenly dispersed therein;

[0058] Step 2: Add 0.02 parts of inhibitor, 10 parts of matting powder, and 13 parts of hydrogenated silicone oil, and stir evenly to disperse the matting powder;

[0059] Step 3: Finally, add 0.5 parts of catalyst and stir evenly to obtain the surface treatment agent.

[0060] The organic silicon leather samples treated with the surface treatment agents obtained in each embodiment and comparative example were prepared as follows: the surface treatment agents prepared in embodiment 1, embodiment 2, comparative example 1 and comparative example 2 were firstly scraped onto the surface of the release paper, with a wet film scraping thickness of 20 μm, and cured at 120° C. for 3 min to obtain a dense treatment layer, and then a 120 μm thick organic silicon intermediate layer (based on weight parts, 100 parts of DY-V401-5000, 5000 viscosity vinyl silicone oil; HB-630 35 parts; DY-V421-1300, 1300 viscosity vinyl silicone oil 5 parts; Delta 2750 silicone resin 30 parts; inhibitor methyl butynol 0.02 parts; catalyst 5000ppm chloroplatinic acid isopropanol solution 0.16 parts; pigment 3 parts (Jiasheng (Shanghai) New Materials, model JSTN207); RH-LHC-3 hydrogenated silicone oil 8 parts; DY-H2O2 hydrogenated silicone oil 4 parts), then cured at 120°C for 3 minutes; finally, apply a silicone top layer (by weight, DY-V401-5000, 5000 viscosity vinyl silicone oil 100 parts; gas silicon HB-630) on the surface of the cured treatment layer. 35 parts; DY-V421-1300, 1300 viscosity vinyl silicone oil 5 parts; Delta 2750 silicone resin 30 parts; inhibitor methyl butynol 0.02 parts; catalyst 5000ppm chloroplatinic acid isopropanol solution 0.16 parts; pigment 3 parts (Jiasheng (Shanghai) New Materials, model JSTN207); RH-LHC-3 hydrogenated silicone oil 8 parts; DY-H2O2 hydrogenated silicone oil 4 parts; tackifier DT-16264 1%) 200μm, and finally bonded to the substrate non-woven fabric, and then placed in an oven at 120°C for complete curing, and finally peeled off the release paper to obtain the silicone leather samples to be tested that were treated with the surface treatment agents of the above embodiments and comparative examples (the sample preparation method is similar to the test sample preparation method of the surface treatment agent for polyurethane leather in the prior art). The silicone leather samples to be tested corresponding to Example 1, Example 2, Comparative Example 1 and Comparative Example 2 were tested according to the following method:

[0061] Feel: touch.

[0062] Abrasion resistance test: Martindale abrasion tester.

[0063] The test is carried out in accordance with GB / T 21196.2. After the test, observe the wear of the surface and record the corresponding number of times.

[0064] The test results are shown in Table 1:

[0065]

[0066] Product 1 and Product 2 in Table 1 are commercially available silicone leather products.

[0067] The other components in the surface treatment agent formula of Example 1 and Example 2 are the same, except that the matting powder used is of different particle sizes. The average particle size of the matting powder in Example 1 is 10 microns, and the average particle size of the matting powder in Example 2 is 2 microns. Through experiments, it is found that when the surface treatment agents of Example 1 and Example 2 are cured at the same wet film coating thickness of 20 μm, the larger the particle size, the drier and smoother it is. The dryness and smoothness of the surface treatment agent prepared by using 10 micron matting powder in Example 1 after coating is significantly better than the dryness and smoothness of the surface treatment agent prepared by using a matting powder with a smaller particle size in Example 2 after coating.

[0068] Comparative Example 1 is completely identical to Example 1 in other conditions, except that the vinyl fluorinated silicone oil of Example 1 is not added. Comparative Example 2 is completely identical to Example 2 in other conditions, except that the vinyl fluorinated silicone oil of Example 2 is not added. The average particle size of the matting powder in Comparative Example 1 is 10 microns, and the average particle size of the matting powder in Example 2 is 2 microns.

[0069] It can be seen that when Comparative Examples 1 and 2 do not contain vinyl fluorinated silicone oil, their wear resistance is significantly reduced compared with Examples 1 and 2, especially when the surface treatment agent of Comparative Example 2 is prepared using a matting powder with a smaller particle size, wear begins to occur after 2,000 frictions, and the wear percentage is as high as 4% after 10,000 frictions. Figure 1 The photos of the silicone leather samples treated with the surface treatment agents of Example 1, Example 2, Comparative Example 1, Comparative Example 2, Commercially Available Product 1 and Commercially Available Product 2 after being rubbed 10,000 times respectively show that the wear resistance of Example 1 and Example 2 is significantly better than that of Comparative Example 1 and Comparative Example 2, and is also significantly better than that of Commercially Available Product 1 and Product 2.

[0070] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A dry and ultra-wear-resistant organic silicon leather surface treatment agent, characterized in that: In parts by weight, it includes: 60-80 parts of vinyl silicone oil; Vinyl fluorosilicone oil 10-15 parts; Polyether modified silicone oil 0.1-1 part; 0.5-2 parts wax powder; Matting powder 10-15 parts; Catalyst 0.2-1 part; 0.02-1 part of inhibitor; and 10-15 parts of hydrogen silicone oil; The viscosity of the vinyl silicone oil is 20000~50000 Pa﹒s; The vinyl fluorosilicone oil has a fluorine content of 10-30% and a vinyl content of 0.0143-0.0184 mol / 100g; the matting powder has a particle size of 10 μm; The polyether-modified silicone oil is synthesized by inserting polyether and alkylene oxide into the chain segments of polymethylsiloxane macromolecules, and has a viscosity of 700-1000 Pa﹒s and an epoxy group content of 1.55-1.9wt%.

2. The surface treatment agent according to claim 1, characterized in that The wax powder is a modified PE wax powder, and its melting point is lower than 120°C.

3. The surface treatment agent according to claim 1, characterized in that The catalyst is a platinum catalyst, and the platinum catalyst is one or more of an isopropanol solution of chloroplatinic acid, a tetrahydrofuran solution of chloroplatinic acid, a chloroplatinic acid-divinyltetramethyldisiloxane complex, chloroplatinic acid-1,3,5,7-tetravinyl-1,3,5,7-tetramethyl-cyclotetrasiloxane, and chloroplatinic acid-divinyltetramethyldisiloxane.

4. The surface treatment agent according to claim 1, characterized in that The hydrogen content of the hydrogen-containing silicone oil is 0.79-1.55 mol / 100 g; the silicon-hydrogen ratio is between 1 and 1.2; and the hydrogen-containing silicone oil comprises side chain hydrogen-containing silicone oil and terminal chain hydrogen-containing silicone oil.

5. The method for preparing a surface treatment agent according to any one of claims 1 to 4, characterized in that: The steps include: (1) Add the vinyl silicone oil, vinyl fluorosilicone oil, polyether modified silicone oil and wax powder in order according to the weight ratio and stir evenly; (2) adding the inhibitor, matting powder and hydrogenated silicone oil and stirring evenly; (3) Finally, the catalyst is added and stirred evenly to obtain the surface treatment agent.

6. Use of the surface treatment agent according to any one of claims 1 to 4 as a silicone leather surface treatment agent.