Environmentally friendly sole rubber composition and preparation method

By adding plant cellulose and photodegradation catalyst to the sole rubber, combined with a specific proportion of rubber materials, the problem of difficult degradation of rubber materials is solved, and efficient degradation within a few years after the end of service life is achieved. The degradation is harmless and maintained. Abrasion resistance and fold resistance of the sole.

CN117887153BActive Publication Date: 2024-11-08GUANGZHOU ZHENGXIN RUBBER & PLASTIC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410136621.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-31
Publication Date
2024-11-08
Estimated Expiration
2044-01-31

AI Technical Summary

Technical Problem

Rubber materials in existing shoe products are difficult to degrade naturally after their service life, resulting in environmental pollution problems.

Method used

Adopt an environmentally friendly sole rubber composition, including butadiene rubber, natural rubber, styrene butadiene rubber, neoprene rubber, carbon black, vegetable oil, composite resin, zinc oxide, stearic acid, accelerator, anti-aging agent, diluting agent and light Degradation catalyst, photodegradation catalyst is prepared by sol-gel method, and combined with plant cellulose, enhance the plasticity and degradability of rubber.

Benefits of technology

The composition can achieve a high degradation rate within a few years after the service life, and the degradation is non-toxic and harmless, solving the problem of environmental pollution of rubber materials, while maintaining the wear and folding resistance of the sole.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004691483500000061
    Figure BDA0004691483500000061
  • Figure BDA0004691483500000071
    Figure BDA0004691483500000071
  • Figure BDA0004691483500000072
    Figure BDA0004691483500000072
Patent Text Reader

Abstract

The present invention provides an environmentally friendly sole rubber composition, which is prepared from raw materials including butadiene rubber, natural rubber, styrene-butadiene rubber, chloroprene rubber, carbon black, vegetable oil, composite resin, zinc oxide, stearic acid, accelerator, antioxidant, repellent, photodegradation catalyst, and plant cellulose. The present invention also discloses a preparation method of the environmentally friendly sole rubber composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber manufacturing, and in particular to an environmentally friendly sole rubber composition and a preparation method thereof. Background Art

[0002] In recent years, with the rapid rise in global temperatures, people's awareness of environmental protection has gradually awakened. Organic pollutants such as plastics and rubber can be seen everywhere in our lives. These pollutants that are difficult to degrade naturally have seriously affected our lives, so we need to take corresponding measures to protect the environment. People's living standards are getting higher and higher, and the quality requirements for footwear products are getting higher and higher. In the shoemaking industry, we often use a large number of high-molecular polymers that are difficult to degrade naturally. Because high-molecular polymers have the advantages of high elasticity, high wear resistance, good softness, acid and alkali resistance, etc., they are widely used in many products. However, this type of high-molecular polymer often contains toxic substances, and the natural degradation is very slow. The toxic substances are released and infiltrated into the soil, causing more serious environmental pollution.

[0003] Vegetable oil is very common in nature. It is not only cheap and has a large output, but also environmentally friendly, non-toxic and renewable. The molecular structure contains unsaturated bonds, which can be grafted onto the main chain of rubber to make the rubber more plastic. In addition, it has a good softening effect on the carbon black in rubber products, enhancing the viscosity of the rubber, making the rubber soft and smooth, and can improve the cold resistance and anti-scorch retardation properties of the products. Its effect on reclaimed rubber: the viscous pine tar absorbs other regeneration agents, and the small molecules in it can evenly penetrate into the middle of the large molecules of the rubber containing sulfur, causing it to swell and relax the network structure, increasing the distance between the molecular chains and the penetration of oxygen. In addition, it can also act as a free radical acceptor, inhibiting gelation, and helping the activator to diffuse into the rubber matrix to accelerate the regeneration process, and can improve the viscosity and plasticity of the reclaimed rubber, with less pollution and good process performance.

[0004] At present, patent application CN110092949B discloses "a rubber composition containing hydrogenated vegetable oil and a preparation method thereof", in which hydrogenated vegetable oil is used as a plasticizer, which has a better plasticizing effect on raw rubber, but the rubber composition has poor degradability and a slow degradation rate.

[0005] In view of the problem in the prior art that the natural degradation rate of organic matter such as rubber after discarded footwear is slow, which seriously pollutes the environment, it is necessary to develop an environmentally friendly material that can decompose quickly after exceeding its service life. Summary of the invention

[0006] Purpose of the invention:

[0007] The purpose of the present invention is to provide an environmentally friendly sole rubber composition, the soles prepared using the composition are durable and can be quickly decomposed after the shoe products exceed their service life, thereby avoiding the problem that the natural degradation rate of organic matter such as rubber is slow after the shoe products are discarded, which seriously pollutes the environment.

[0008] The technical solution of the present invention:

[0009] An environmentally friendly sole rubber composition, comprising the following components in parts by weight:

[0010] 30-60 parts of butadiene rubber;

[0011] 20-50 parts of natural rubber;

[0012] 30-45 parts of styrene-butadiene rubber;

[0013] 40-55 parts of chloroprene rubber;

[0014] Carbon black 5-10 parts;

[0015] 2-5 parts vegetable oil;

[0016] 3-5 parts of composite resin;

[0017] 3-8 parts of zinc oxide;

[0018] 0.8-1.5 parts of stearic acid;

[0019] 1 to 3 parts of accelerator;

[0020] 1 to 3 parts of antioxidant;

[0021] 1 to 3 parts of thinning agent;

[0022] 2 to 7 parts of photodegradation catalyst;

[0023] 20-30 parts of plant cellulose.

[0024] Preferably, the environmentally friendly sole rubber composition is characterized in that, in parts by weight, the environmentally friendly sole rubber composition comprises the following components:

[0025] 45-50 parts of butadiene rubber;

[0026] 35-40 parts of natural rubber;

[0027] 37-40 parts of styrene-butadiene rubber;

[0028] 48-52 parts of chloroprene rubber;

[0029] Carbon black 5-10 parts;

[0030] 3-4 parts vegetable oil;

[0031] 3-5 parts of composite resin;

[0032] 3-8 parts of zinc oxide;

[0033] 0.8-1.5 parts of stearic acid;

[0034] 1 to 3 parts of accelerator;

[0035] 1 to 3 parts of antioxidant;

[0036] 1 to 3 parts of thinning agent;

[0037] 3-5 parts of photodegradation catalyst;

[0038] 25-30 parts of plant cellulose.

[0039] Preferably, the vegetable oil is one or more of industrial grade palm oil, linseed oil, and tung seed oil.

[0040] Preferably, the mass ratio of the industrial-grade palm oil, linseed oil and tung seed oil is 1:1-1.5:1-2.

[0041] The preparation method of the photodegradation catalyst comprises the following steps:

[0042] (1) Preparation of CsBr-TiO by sol-gel method 2 Gel: Add butyl titanate to anhydrous ethanol, stir for 10 to 20 minutes, then add glacial acetic acid and stir to obtain solution A;

[0043] (2) Take nitric acid solution, add it to anhydrous ethanol, stir evenly, and obtain solution B;

[0044] (3) Solution B is added dropwise to solution A slowly, and stirred for 1 to 2 hours after the addition is complete. Then cesium bromide is added and magnetically stirred until a transparent gel is formed. The resulting gel is allowed to stand at room temperature, dried, ground, calcined, and then cooled to room temperature to obtain a photodegradation catalyst.

[0045] Preferably, the mass ratio of butyl titanate to cesium bromide is 2 to 8:1.

[0046] Preferably, the plant cellulose is one or more of coffee fiber, wood fiber and ramie fiber.

[0047] Preferably, the mass ratio of the coffee fiber, the wood fiber and the ramie fiber is 1-2:1-1.5:1.

[0048] Preferably, the mass ratio of the vegetable oil, the photodegradation catalyst and the plant cellulose is 1:1-2:6-10.

[0049] The present application also provides a method for preparing an environmentally friendly sole rubber composition, which is characterized by comprising the following steps:

[0050] (1) adding butadiene rubber, natural rubber, styrene-butadiene rubber (SBR), and chloroprene rubber (CR) in order according to the formula weight into a low-speed mixer, and mixing to obtain a mixture;

[0051] (2) adding the mixture obtained in step (1) into an internal mixer for main rubber mixing;

[0052] (3) adding vegetable oil and part of carbon black, composite resin, zinc oxide, and stearic acid to the mixture in step (2) and mixing them in an internal mixer, and then adding part of accelerator, antioxidant, vulcanizing agent, and plant cellulose to the internal mixer and mixing them;

[0053] (4) adding the photodegradation catalyst and the remaining carbon black, composite resin, zinc oxide, and stearic acid to the step (3) into an internal mixer and mixing, and then adding the remaining accelerator, antioxidant, vulcanizing agent, and plant cellulose into the internal mixer and mixing;

[0054] (5) plasticizing and extruding the mixture after banburying in step (4) using a screw extruder, and cooling after extrusion;

[0055] (6) After the product obtained in step (5) is hardened, it is granulated using a pelletizer, and the pellets are placed in a vulcanizer for vulcanization, and the vulcanization temperature is set to control the vulcanization time;

[0056] (7) After the material of step (6) is vulcanized, it is placed at room temperature for 5 to 8 hours, and the granules are added to an open mill, and then molded to form a finished product.

[0057] Preferably, in step 1, the mixing speed is 150-200 rpm and the mixing time is 10-20 minutes; in step 2, the mixing temperature is 60-80°C and the time is 5-8 minutes; in step 3, the mixing temperature is 80-100°C and the time is 2-5 minutes; in step 4, the mixing temperature is 100-130°C and the time is 5-10 minutes; in step 5, the temperatures of the five temperature zones in the extruder are set to 120°C, 130°C, 140°C, 130°C and 140°C respectively, the main engine speed is 400-500 rpm, and the extrudate is cooled at 10-20°C; in step 6, the vulcanization temperature is 140-160°C and the vulcanization time is 3-5 minutes.

[0058] Preferably, the composite resin is a mixture of terpene resin, phenolic resin and vinyl acetate in a mass ratio of 1 to 1.2:1:1 to 1.4.

[0059] Preferably, the accelerator is a mixture of DOTG, 2-mercaptobenzothiazole and TMTD in a mass ratio of 1 to 1.5:1:1 to 1.2.

[0060] Preferably, the antioxidant is a mixture of RD (2,2,4-trimethyl-1,2-dihydropyrrolidone polymer), ODA (4,4'-dioctyldiphenylamine) and MB (2-mercaptobenzimidazole) in a mixing ratio of 1 to 2:1 to 1.5:1.

[0061] Preferably, the vulcanizing agent is a mixture of sulfur, bismaleimide and dicumyl peroxide in a mass ratio of 2:1 to 1.2:1 to 1.2.

[0062] The grafting of vegetable oil and rubber enhances the plasticity and elasticity of the rubber. The plant cellulose is degradable and has certain toughness, wear resistance and hardness, making the rubber not easy to break. It has good softness, ductility and flexibility, and can withstand multiple bending, stretching and compression without being damaged. It has high acid and alkali resistance and can maintain the beautiful appearance of the product. The photodegradation catalyst is added to the rubber composition to make the rubber photodegradable, and the proportion of the photodegradation catalyst to the vegetable oil and the plant cellulose is controlled, so that the prepared sole rubber composition has good durability and can achieve a good degradation rate within a few years after exceeding the service life, and the degradation products are non-toxic and harmless, and are environmentally friendly.

[0063] Beneficial effects:

[0064] The environmentally friendly sole rubber composition provided by the invention is added with vegetable oil and vegetable cellulose, so that the plasticity, elasticity and wear resistance of the rubber are enhanced, the rubber is not easy to break, can withstand multiple bending, stretching and compression without being damaged, and has high acid and alkali resistance; a photodegradation catalyst is added to enable the rubber to undergo a photodegradation reaction, and the proportion of the photodegradation catalyst to the vegetable oil and the vegetable cellulose is controlled, so that a good degradation rate can be achieved within a few years after the shoe products are discarded, thereby solving the problem that the natural degradation rate of organic matter such as rubber is slow after the shoe products are discarded, which seriously pollutes the environment. DETAILED DESCRIPTION

[0065] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0066] Unless otherwise specified, the chemical reagents used in the present invention are all commercially available analytically pure. Aromatic oil was purchased from Hengshui Diyi Petrochemical Co., Ltd., model G17; other photocatalysts were purchased from Leiyang Taitang Technology Co., Ltd. Nano-titanium dioxide colloid, CAS No.: 13463-67-7; terpene resin, phenolic resin and vinyl acetate resin were purchased from Shanghai Sanlian Industrial Co., Ltd.; antioxidants RD, ODA, MB were purchased from Jinan Xinrui Rubber and Plastic Technology Co., Ltd., CAS Nos.: 26780-96-1, 101-67-7, 583-39-1, respectively; butadiene rubber, natural rubber, Styrene-butadiene rubber was purchased from Xiamen Mingjia New Materials Co., Ltd.; chloroprene rubber was purchased from Dongguan Futai Rubber Co., Ltd., model Changshou CR2444; industrial-grade palm oil was purchased from Shandong Youwang Chemical Products Co., Ltd.; linseed oil was purchased from Heze Zhonghe Jianyuan Biotechnology Co., Ltd.; tung seed oil was purchased from Jinan Lianshun Chemical Co., Ltd.; offee fiber was purchased from Dongguan Baida Plastic Raw Materials Co., Ltd.; wood fiber was purchased from Shandong Binli New Materials Co., Ltd.; ramie fiber was purchased from Linyi Yuanma Crafts Co., Ltd.; aromatic oil was purchased from Jinan Xinhaoyuan Chemical Co., Ltd., model KN-4006; soybean oil was purchased from Shandong Defa Chemical Co., Ltd.

[0067] Preparation of photodegradation catalyst A:

[0068] (1) Preparation of CsBr-TiO by sol-gel method 2 Gel: Add 5g of butyl titanate to 30ml of anhydrous ethanol, stir for 10min, then add 5ml of glacial acetic acid and stir to obtain solution A;

[0069] (2) Take 6 mL of 1.6 mol / L nitric acid solution, add it to 8 mL of anhydrous ethanol, and stir magnetically for 30 min to form solution B;

[0070] (3) Solution B was added dropwise to solution A for 20 min, and stirring was continued for 1 h. Then, 1 g of cesium bromide was added and magnetic stirring was performed until a transparent gel was formed. The resulting gel was allowed to stand at room temperature for 12 h, dried at 90 °C for 18 h, ground, and then calcined at 500 °C for 6 h. The photodegradation catalyst A was obtained by cooling.

[0071] Preparation of photodegradation catalyst B:

[0072] (1) Preparation of CsBr-TiO by sol-gel method 2 Gel: Add 1g of butyl titanate to 30ml of anhydrous ethanol, stir for 10min, then add 5ml of glacial acetic acid and stir to obtain solution A;

[0073] (2) Take 6 mL of 1.6 mol / L nitric acid solution, add it to 8 mL of anhydrous ethanol, and stir magnetically for 30 min to form solution B;

[0074] (3) Solution B was added dropwise to solution A for 20 min, and stirring was continued for 1 h. Then, 1 g of cesium bromide was added and magnetic stirring was performed until a transparent gel was formed. The resulting gel was allowed to stand at room temperature for 12 h, dried at 90 °C for 18 h, ground, and then calcined at 500 °C for 6 h. The photodegradation catalyst B was obtained by cooling.

[0075] Preparation of environmentally friendly sole rubber composition:

[0076] (1) adding butadiene rubber, natural rubber, styrene-butadiene rubber and chloroprene rubber in order according to the formula weight into a low-speed mixer, mixing at 150 rpm and room temperature for 15 minutes to obtain a mixture;

[0077] (2) adding the mixture obtained in step (1) into an internal mixer to mix the main rubber at a mixing temperature of 75° C. for 5 minutes;

[0078] (3) adding vegetable oil and half of the carbon black, composite resin (a mixture of terpene resin, phenolic resin and vinyl acetate in a mass ratio of 1:1:1), zinc oxide and stearic acid to step (2) and mixing at a mixing temperature of 90°C for 5 minutes, and then adding half of the accelerator (a mixture of DOTG, 2-mercaptobenzothiazole and TMTD in a mass ratio of 1:1:1), antioxidant (a mixture of RD, ODA and MB in a mass ratio of 2:1:1), vulcanizing agent (a mixture of sulfur, bismaleimide and diisopropylbenzene peroxide in a mass ratio of 2:1:1), and plant cellulose to a mixer, mixing at a mixing temperature of 80°C for 5 minutes;

[0079] (4) adding the photodegradation catalyst and the remaining carbon black, composite resin, zinc oxide, and stearic acid to the step (3) into an internal mixer and mixing at a mixing temperature of 120° C. for 8 minutes, and then adding the remaining accelerator, antioxidant, vulcanizing agent, and plant cellulose into an internal mixer and mixing at a mixing temperature of 120° C. for 10 minutes;

[0080] (5) plasticizing and extruding the mixture after banburying in step (4) by a screw extruder, wherein the five temperature zones in the extruder are set to 120° C., 130° C., 140° C., 130° C., and 140° C., respectively, and the main engine speed is 450 rpm, and the extrudate is cooled at 15° C.;

[0081] (6) After the product obtained in step (5) is hardened, it is pelletized using a pelletizer, and the pellets are placed in a vulcanizer for vulcanization at a vulcanization temperature of 150° C. for 5 minutes;

[0082] (7) The material of step (6) is vulcanized and placed at room temperature for 6 hours, the pellets are added to an open mixing mill, and then molded to form a finished product.

[0083] Examples 1 to 9

[0084] The environmentally friendly sole rubber composition was prepared according to the above-mentioned preparation method. Table 1 is the ingredient list of the environmentally friendly sole rubber composition of Examples 1 to 9.

[0085] Table 1 Ingredients of environmentally friendly sole rubber compositions of Examples 1 to 9

[0086]

[0087]

[0088] Comparative Examples 1 to 4 were prepared according to the above-mentioned preparation method of the environmentally friendly sole rubber composition. Table 2 is the ingredient list of the environmentally friendly sole rubber composition of Comparative Examples 1 to 4.

[0089] Table 2 Ingredients of environmentally friendly sole rubber compositions of comparative examples 1 to 4

[0090]

[0091]

[0092] Performance test experiment:

[0093] 1. Wear resistance test:

[0094] According to the GB-9867-1988 standard, the rubber composition is tested for soles. After a certain distance of wear, the surface wear condition, weight loss, volume loss, wear thickness and other characteristics of the sample are evaluated. The wear resistance is evaluated by comparison with the standard rubber.

[0095] 2. Folding resistance test: According to the “General Test Method for Folding Resistance of Footwear”, the rubber composition is made into a sole and flexed continuously for 50,000 to 70,000 times at a temperature of 23°C.

[0096] 3. Cut the rubber shoe products into 2*2mm sheet specimens, weigh the initial weight of each sheet, spread them flat in the sample box, place them in a dark environment for 30 minutes, and then move them under a MICROSOLAR300 light source for irradiation. Take a sample every 3 hours, measure its weight, and calculate the photodegradation rate of the rubber product based on the weight change.

[0097] Table 3: Performance test results

[0098]

[0099]

[0100] It can be seen from Table 3 that the environmentally friendly sole rubber composition of the present invention contains vegetable oil and a photodegradation catalyst, which makes the rubber sole have better wear resistance and folding resistance, and has a good degradation rate under simulated 5-year light intensity irradiation. Specifically, by comparing Example 4 with Example 2, it can be seen that an unreasonable mass ratio of industrial-grade palm oil, linseed oil, and tung seed oil in vegetable oil will lead to poor wear resistance of the rubber composition; by comparing Example 5 with Example 2 and Example 4, it can be seen that the use of other photodegradation catalysts on the market will lead to poor photodegradability of the rubber composition; by comparing Example 6 with Example 2, it can be seen that the rubber composition prepared by using plant cellulose with an unreasonable mass ratio of offee fiber, wood fiber, and ramie fiber has poor flexural wear resistance; by comparing Example 7 with Example 1, it can be seen that the rubber composition containing industrial-grade palm oil, linseed oil, and tung seed oil (mass ratio of 1:1:1) has better wear resistance and degradation rate than the rubber composition containing soybean oil; by comparing Example 8 with Examples 1-3, it can be seen that an unreasonable mass ratio of photodegradation catalyst, vegetable oil, and plant cellulose will lead to poor wear resistance and folding resistance of the rubber composition, low photodegradation rate, and fail to achieve the expected effect; by comparing Example 9 with Example 2, it can be seen that the rubber composition using a photodegradation catalyst prepared with an unreasonable weight ratio of cesium bromide to butyl titanate has poor photodegradability. From the comparison between Comparative Example 1 and Example 2, it can be seen that the rubber composition containing industrial-grade palm oil, linseed oil and tung seed oil (mass ratio is 1:1:1) has better wear resistance, folding resistance and degradation rate than the rubber composition containing aromatic oil; from the comparison between Comparative Example 2 and Example 2, it can be seen that the rubber composition not containing vegetable oil has a low photodegradation rate; from the comparison between Comparative Example 3 and Example 2, it can be seen that the rubber composition not containing a photodegradation catalyst has low wear resistance, folding resistance and degradation rate; from the comparison between Comparative Example 4 and Example 3, it can be seen that the rubber composition not containing both vegetable oil and photodegradation catalyst has poor wear resistance and folding resistance, low photodegradation rate, and cannot achieve the expected effect.

[0101] The present invention can also have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. An environmentally friendly sole rubber composition, which comprises the following components in parts by weight: 30~60 parts of butadiene rubber; 20~50 parts of natural rubber; 30-45 parts of styrene-butadiene rubber; 40~55 parts of chloroprene rubber; Carbon black 5-10 parts; 2-5 parts vegetable oil; 3~5 parts of composite resin; 3-8 parts of zinc oxide; 0.8-1.5 parts of stearic acid; 1~3 parts of accelerator; 1~3 parts of antioxidant; 1~3 parts of thinning agent; 2-7 parts of photodegradation catalyst; 20-30 parts of plant cellulose; The preparation method of the photodegradation catalyst comprises the following steps: (1) Preparation of CsBr-TiO2 gel by sol-gel method: Add butyl titanate to anhydrous ethanol, stir for 10-20 min, then add glacial acetic acid and stir to obtain solution A; (2) Take nitric acid solution, add it to anhydrous ethanol, stir evenly, and obtain solution B; (3) Add solution B to solution A slowly, stir for 1-2 hours after the addition is complete, then add cesium bromide and stir magnetically until a transparent gel is formed. The resulting gel is allowed to stand at room temperature, dried, ground, calcined, and then cooled to room temperature to obtain a photodegradation catalyst. The mass ratio of butyl titanate to cesium bromide is 2-8:1; The vegetable oil is industrial grade palm oil, linseed oil, or tung seed oil; The mass ratio of the industrial grade palm oil, linseed oil and tung seed oil is 1:1-1.5:1-2.

2. The environmentally friendly sole rubber composition according to claim 1, characterized in that: The environmentally friendly sole rubber composition comprises the following components in parts by weight: 45-50 parts of butadiene rubber; 35~40 parts of natural rubber; Styrene butadiene rubber 37-40 parts; Neoprene 48-52 parts; Carbon black 5-10 parts; 3-5 parts vegetable oil; 3~5 parts of composite resin; Zinc oxide 4-7 parts; 0.8-1.5 parts of stearic acid; 1~3 parts of accelerator; 1~3 parts of antioxidant; 1~3 parts of thinning agent; 3-5 parts of photodegradation catalyst; 25-30 parts of plant cellulose.

3. The environmentally friendly sole rubber composition according to claim 1, characterized in that: The plant cellulose is one or more of coffee fiber, wood fiber and ramie fiber.

4. The environmentally friendly sole rubber composition according to claim 3, characterized in that: The mass ratio of the coffee fiber, the wood fiber and the ramie fiber is 1-2:1-1.5:

1.

5. The environmentally friendly sole rubber composition according to claim 1, characterized in that: The mass ratio of the vegetable oil, the photodegradation catalyst and the plant cellulose is 1:1-1.5:6-10.

6. The method for preparing the environmentally friendly sole rubber composition according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) adding butadiene rubber, natural rubber, styrene-butadiene rubber and chloroprene rubber into a low-speed mixer in order according to the formula weight, and mixing to obtain a mixture; (2) adding the mixture obtained in step (1) into an internal mixer for main rubber mixing; (3) adding vegetable oil and half of the carbon black, composite resin, zinc oxide, and stearic acid in step (2) into an internal mixer and mixing, and then adding half of the accelerator, antioxidant, vulcanizing agent, and plant cellulose into the internal mixer and mixing; (4) adding the photodegradation catalyst and the remaining carbon black, composite resin, zinc oxide, and stearic acid in step (3) into an internal mixer and mixing them, and then adding the remaining accelerator, antioxidant, vulcanizing agent, and plant cellulose into the internal mixer and mixing them; (5) plasticizing and extruding the mixture after the banburying in step (4) using a screw extruder, and cooling after extrusion; (6) After the product obtained in step (5) is hardened, it is pelletized using a pelletizer, and the pellets are placed in a vulcanizer for vulcanization, and the vulcanization temperature is set to control the vulcanization time; (7) After the material in step (6) is vulcanized, it is placed at room temperature for 5 to 8 hours, the pellets are added to an open mill, and then molded to form a finished product.