A wear-resistant seamless steel pipe perforation plug and a preparation method thereof
By optimizing the composition and process of the seamless steel pipe perforated plug, and combining it with plasma spraying technology to form a zirconium-chromium coating, the problem of insufficient wear resistance and temperature resistance of the plug is solved, achieving higher wear resistance and high temperature resistance, and extending the Extended service life and reduced costs.
Patent Information
- Application Number
- CN202410357567.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-03-27
AI Technical Summary
The existing perforated plugs of seamless steel pipes have insufficient wear resistance and temperature resistance in high temperature, high pressure, and rapid cooling and heating environments, resulting in short service life, high cost, and ineffective traditional protective measures.
By optimizing the composition of the plug, adding molten steel purifier, using annealing, quenching, tempering processes and non-hydrolytic sol-gel method to prepare chromium-zirconium powder, and forming a zirconium-chromium coating with a thickness of 1-5mm through plasma spraying technology, improving The wear resistance and high temperature resistance of the head.
The wear resistance and high temperature resistance of the seamless steel pipe perforated plug are significantly improved, the service life is extended, the process is simplified and the cost is reduced, and the hardness and toughness of the plug are enhanced.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal materials, in particular to a wear-resistant seamless steel pipe perforation plug and a preparation method thereof. Background Art
[0002] The seamless steel pipe industry accounts for an important part of the national economy, and the perforated plug is one of the most consumed key tools in the production of seamless steel pipes. During the pipe-piercing process, the perforated plug is in direct contact with the high-temperature steel billet. During the final rolling, the nose temperature of the plug is as high as about 1300℃, and it is subjected to huge axial pressure, radial stress and surface friction. Moreover, each time the perforated plug is completed, it must be forced to be water-cooled. In the harsh working environment of high temperature, high pressure and rapid cooling and heating, it is subjected to the combined effects of mechanical fatigue and thermal fatigue, which causes the perforated plug to fail in the form of nose collapse, steel sticking and cracking earlier, which seriously affects the output, quality and economic benefits of steel pipe production. Therefore, the development of a high-quality perforated plug has become an important issue in steel pipe production.
[0003] Traditional plug materials are made of high-alloy die steel or molybdenum alloy. Although high-alloy die steel has high hardness and strength at high temperatures, it is easy to crack in a rapid cooling and heating working environment and has a short service life. Molybdenum alloy plug materials are expensive and not suitable for large-scale use. At present, the protection of plug materials mainly adopts pre-oxidation treatment to preform an iron oxide film on the plug surface to prevent the plug substrate from directly contacting the tube blank, which plays a certain role in heat insulation. However, due to the loose structure and easy cracking of the iron oxide film, its oxidation resistance, adhesion and high-temperature stability are poor. Therefore, pre-oxidation treatment is difficult to effectively solve the industry problem of rapid failure of the plug. Patent No. CN101603154A discloses a new material for hot perforation plugs of steel pipes. The content of Mo and W is appropriately increased on the basis of low alloy, and Al and rare earth element Ce are added. Compared with high alloy steel, the cost is lower. The new material improves the hardness, strength, toughness and other properties of the new material of the perforation plug to a certain extent, but its wear resistance and temperature resistance are not significantly improved, so that the service life of the perforation plug is not long.
[0004] The perforating plug is a consumable with a complicated manufacturing process and a high manufacturing cost. Preparing a protective coating on the surface of the plug is an effective method to protect the plug and ensure its dimensional accuracy. The present invention optimizes the components of the plug, adds an appropriate amount of molten steel purifier, improves the cleanliness, reduces the amount of precious alloy elements, and saves costs. Then, a suitable annealing, quenching, and tempering process is used for heat treatment, and a chromium-zirconium powder with excellent wear resistance is prepared by a non-hydrolytic sol-gel method. The surface is treated by plasma spraying to obtain a wear-resistant and high-temperature resistant seamless steel pipe perforating plug. Summary of the invention
[0005] The technical problem solved by the invention is to provide a wear-resistant seamless steel pipe perforation plug and a preparation method thereof, thereby solving the problem that the existing seamless steel pipe perforation plug has poor wear resistance and high temperature resistance.
[0006] The technical solution of the present invention is:
[0007] A wear-resistant seamless steel pipe perforated plug comprises the following components in percentage by mass: 0.28-0.42% pure carbon, 0.45-0.78% pure silicon, 0.31-0.52% metallic manganese, 1.85-2.63% metallic chromium, 0.33-0.54% metallic vanadium, 2.23-2.89% metallic nickel, 0.15-0.25% metallic tungsten, 0.01-0.1% pure nitrogen, 0.03-0.15% molten steel purifier, and the balance is metallic iron.
[0008] The preparation method of the wear-resistant seamless steel pipe perforation plug is carried out according to the following steps:
[0009] (1) Preparation of seamless steel pipe perforated plug matrix: Add the above-mentioned components in a medium frequency induction furnace, heat and smelt them, and after they are completely melted, pour them into a preheated stainless steel mold, evacuate them for vacuum casting, and place them in a muffle furnace at 500-650°C for 30-50 minutes after molding to obtain a seamless steel pipe perforated plug matrix.
[0010] (2) Preparation of the seamless steel pipe perforated plug pre-finished product: The seamless steel pipe perforated plug substrate is placed in a muffle furnace, heated at a rate of 3-6°C / min for quenching, then cooled at a rate of 6-10°C / min for tempering, and air-cooled after being taken out of the furnace to obtain the seamless steel pipe perforated plug pre-finished product.
[0011] (3) Preparation of zirconium-chromium powder: Add zirconium chloride and anhydrous ethanol to a reaction flask, mix well, then add chromium carbonate and stir to react. After the reaction is completed, vacuum distillation is performed to obtain white sandy particles, which are then calcined at 600-800°C for 1-3 hours and cooled to room temperature to obtain zirconium-chromium powder.
[0012] (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. The powder feeding gas feeds zirconium-chromium powder from the nozzle into the plasma jet, heats it to a molten state, and sprays it onto the surface of the seamless steel pipe perforated plug, forming a zirconium-chromium coating with a thickness of 1-5 mm to obtain a wear-resistant seamless steel pipe perforated plug.
[0013] Furthermore, the molten steel purifier is any one of magnesium-cerium alloy, rhenium-magnesium alloy or lanthanum-aluminum alloy.
[0014] Furthermore, in step (1), the smelting temperature is 950-1100° C. and the smelting time is 1-3 h.
[0015] Furthermore, in step (2), the quenching temperature is 900-1050°C and the quenching time is 3-6h.
[0016] Furthermore, in step (2), the tempering temperature is 550-700° C., and the tempering time is 1-4 h.
[0017] Furthermore, in step (3), the ratio of zirconium chloride to chromium carbonate is 1 mol: (1.1-1.4) mol.
[0018] Furthermore, in step (3), the reaction temperature is 60-70° C. and the reaction time is 5-10 h.
[0019] Furthermore, in step (4), the powder feeding gas is any one of argon, hydrogen, helium and nitrogen.
[0020] Furthermore, in step (4), the spraying power of the plasma spray gun is 25-35 kW, the operating voltage is 55-65 V, and the operating current is 450-550 A.
[0021] Furthermore, in step (4), the powder feeding gas flow rate is 280-320 L / h, and the powder feeding speed is 5-8 g / min.
[0022] The beneficial technical effects of the present invention are:
[0023] The present invention optimizes the design of the components of the seamless steel pipe perforation plug, adds a proper amount of molten steel purifier, reduces the amount of precious alloy elements, and strengthens the metal material; adopts appropriate annealing, quenching, tempering and other heat treatment processes, adopts a non-hydrolytic sol-gel method to prepare chromium zirconium powder with excellent wear resistance for the primary finished product of the seamless steel pipe perforation plug, and plasma sprays the surface of the seamless steel pipe perforation plug to obtain a wear-resistant seamless steel pipe perforation plug, thereby simplifying the process and reducing the cost.
[0024] The rare earth elements in the molten steel purifier react with O and S in the molten steel to generate rare earth oxides, rare earth sulfur oxides and rare earth sulfide inclusions, reducing the content of O and S in the molten steel. The dispersed small spherical rare earth sulfide inclusions can replace the long strip MnS inclusions in the steel, improving the toughness and corrosion resistance of the steel. At the same time, the deoxidation ability of magnesium and aluminum is significantly stronger than the desulfurization ability. The synergistic treatment of magnesium-cerium alloy can change the type of inclusions in the molten steel, reduce the ability of inclusions to aggregate and float, and improve the purification degree of the molten steel. Then, fine and dispersed high-melting point compounds are precipitated before the molten steel solidifies, reducing the supercooling of the molten steel, refining the grains after the molten steel solidifies, and improving the strength of the steel. In addition, the radius of rare earth elements is large and it is difficult to diffuse in the grains. The rare earth atoms concentrated at the grain boundaries can also play a pinning role on the grain boundaries, thereby improving the hardness of the piercing head.
[0025] The zirconium-chromium coating has zirconium and chromium with excellent wear resistance, which can be used as a hard phase. During the friction and wear process, it can effectively resist the wear of external abrasive particles. The crack source and crack propagation path of wear microcracks generated during wear are greatly restricted, and the sliding friction and chiseling of some abrasive particles on the coating surface can be transformed into rolling, which reduces the wear of the coating by the abrasive particles, thereby improving the wear resistance of the perforated head of the seamless steel pipe; plasma spraying heats the thermal spraying material to a plastic or molten state, and then accelerates it with compressed air, so that the constrained particle beam impacts the surface of the substrate. The particles impacting the surface are deformed due to stamping to form laminated thin sheets, which adhere to the prepared substrate surface, and then cool and accumulate continuously, finally forming a layered coating, realizing the high temperature resistance and wear resistance of the perforated head material. DETAILED DESCRIPTION
[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example
[0027] (1) Preparation of seamless steel pipe perforated plug matrix: 0.31% pure carbon, 0.52% pure silicon, 0.35% metal manganese, 2.24% metal chromium, 0.46% metal vanadium, 2.58% metal nickel, 0.20% metal tungsten, 0.03% pure nitrogen, 0.03% magnesium-cerium alloy, and the balance metal iron are added to a medium frequency induction furnace, heated to 1050°C and smelted for 2 h. After being completely melted, it is poured into a preheated stainless steel mold and vacuumed for vacuum casting. After molding, it is placed in a muffle furnace at 550°C and kept warm for 40 min to obtain a seamless steel pipe perforated plug matrix.
[0028] (2) Preparation of the seamless steel pipe perforated plug pre-finished product: The seamless steel pipe perforated plug substrate is placed in a muffle furnace, heated to 1000°C at a rate of 5°C / min, quenched for 5 h, then cooled to 650°C at a rate of 8°C / min and tempered for 3 h. The substrate is then taken out of the furnace and air-cooled to obtain the seamless steel pipe perforated plug pre-finished product.
[0029] (3) Preparation of zirconium-chromium powder: Add 5 mmol of zirconium chloride and 40 mL of anhydrous ethanol to a reaction flask. After mixing evenly, add 6.2 mmol of chromium carbonate. React at 65°C for 9 h. Vacuum distillation is performed to obtain white sandy particles. Then, the particles are calcined at 700°C for 2 h and cooled to room temperature to obtain zirconium-chromium powder.
[0030] (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The spraying power is 30 kW, the working voltage is 60 V, and the working current is 500 A. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. Argon gas is used to send zirconium-chromium powder from the nozzle into the plasma jet at a flow rate of 310 L / h and a speed of 6 g / min. It is heated to a molten state and sprayed onto the surface of the seamless steel pipe perforated plug to form a zirconium-chromium coating with a thickness of 1 mm to obtain a wear-resistant seamless steel pipe perforated plug. Example
[0031] (1) Preparation of seamless steel pipe perforated plug matrix: 0.28% pure carbon, 0.78% pure silicon, 0.52% metal manganese, 1.85% metal chromium, 0.54% metal vanadium, 2.89% metal nickel, 0.15% metal tungsten, 0.07% pure nitrogen, 0.06% rhenium magnesium alloy, and the balance metal iron are added to a medium frequency induction furnace, heated to 1100°C and smelted for 1 h. After being completely melted, they are poured into a preheated stainless steel mold, vacuumed for vacuum casting, and placed in a muffle furnace at 650°C for 30 min after forming to obtain a seamless steel pipe perforated plug matrix.
[0032] (2) Preparation of the seamless steel pipe perforated plug pre-finished product: The seamless steel pipe perforated plug substrate is placed in a muffle furnace, heated to 1050°C at a rate of 6°C / min and quenched for 3 h, then cooled to 700°C at a rate of 10°C / min and tempered for 1 h. The substrate is then air-cooled to obtain the seamless steel pipe perforated plug pre-finished product.
[0033] (3) Preparation of zirconium-chromium powder: Add 12 mmol of zirconium chloride and 60 mL of anhydrous ethanol to a reaction flask. After mixing evenly, add 13.2 mmol of chromium carbonate. React at 70°C for 5 h. Vacuum distillation is performed to obtain white sandy particles. The particles are then calcined at 800°C for 1 h and cooled to room temperature to obtain zirconium-chromium powder.
[0034] (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The spraying power is 35 kW, the working voltage is 55 V, and the working current is 450 A. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. Hydrogen gas feeds zirconium-chromium powder from the nozzle into the plasma jet at a flow rate of 320 L / h and a speed of 8 g / min. It is heated to a molten state and sprayed onto the surface of the seamless steel pipe perforated plug to form a zirconium-chromium coating with a thickness of 1 mm to obtain a wear-resistant seamless steel pipe perforated plug. Example
[0035] (1) Preparation of seamless steel pipe perforated plug matrix: 0.42% pure carbon, 0.45% pure silicon, 0.31% metal manganese, 2.63% metal chromium, 0.33% metal vanadium, 2.23% metal nickel, 0.25% metal tungsten, 0.1% pure nitrogen, 0.09% lanthanum aluminum alloy, and the balance metal iron are added to a medium frequency induction furnace, heated to 950°C and smelted for 3 hours. After being completely melted, it is poured into a preheated stainless steel mold and vacuumed for vacuum casting. After molding, it is placed in a muffle furnace at 500°C and kept warm for 50 minutes to obtain a seamless steel pipe perforated plug matrix.
[0036] (2) Preparation of the seamless steel pipe perforated plug pre-finished product: The seamless steel pipe perforated plug substrate is placed in a muffle furnace, heated to 900°C at a rate of 3°C / min, quenched for 6 h, then cooled to 550°C at a rate of 6°C / min, tempered for 4 h, and air-cooled to obtain the seamless steel pipe perforated plug pre-finished product.
[0037] (3) Preparation of zirconium-chromium powder: Add 8 mmol of zirconium chloride and 80 mL of anhydrous ethanol into a reaction flask and mix well. Then add 11.2 mmol of chromium carbonate and react at 60°C for 10 h. Distill under reduced pressure to obtain white sandy particles. Then calcine at 600°C for 3 h and cool to room temperature to obtain zirconium-chromium powder.
[0038] (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The spraying power is 25 kW, the working voltage is 65 V, and the working current is 550 A. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. Helium gas is used to feed zirconium-chromium powder from the nozzle into the plasma jet at a flow rate of 280 L / h and a speed of 5 g / min. It is heated to a molten state and sprayed onto the surface of the seamless steel pipe perforated plug to form a zirconium-chromium coating with a thickness of 1 mm to obtain a wear-resistant seamless steel pipe perforated plug. Example
[0039] (1) Preparation of seamless steel pipe perforated plug matrix: 0.35% pure carbon, 0.62% pure silicon, 0.49% metallic manganese, 2.25% metallic chromium, 0.42% metallic vanadium, 2.66% metallic nickel, 0.18% metallic tungsten, 0.08% pure nitrogen, 0.12% magnesium-cerium alloy, and the balance metallic iron are added into a medium frequency induction furnace, heated to 1080°C and smelted for 2 h. After being completely melted, the mixture is poured into a preheated stainless steel mold, vacuumed for vacuum casting, and placed in a muffle furnace at 560°C for 45 min to obtain a seamless steel pipe perforated plug matrix.
[0040] (2) Preparation of the seamless steel pipe perforated plug pre-finished product: The seamless steel pipe perforated plug substrate is placed in a muffle furnace, heated to 980°C at a rate of 4°C / min, quenched for 6 h, then cooled to 650°C at a rate of 8°C / min, tempered for 3 h, and air-cooled to obtain the seamless steel pipe perforated plug pre-finished product.
[0041] (3) Preparation of zirconium-chromium powder: Add 3 mmol of zirconium chloride and 27 mL of anhydrous ethanol to a reaction flask. After mixing evenly, add 3.78 mmol of chromium carbonate. React at 70°C for 8 h. Vacuum distillation is performed to obtain white sandy particles. The particles are then calcined at 720°C for 3 h and cooled to room temperature to obtain zirconium-chromium powder.
[0042] (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the pre-finished product of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The spraying power is 28 kW, the working voltage is 62 V, and the working current is 520 A. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. Nitrogen feeds zirconium-chromium powder from the nozzle into the plasma jet at a flow rate of 300 L / h and a speed of 6 g / min. It is heated to a molten state and sprayed onto the surface of the pre-finished product of the seamless steel pipe perforated plug to form a zirconium-chromium coating with a thickness of 1 mm to obtain a wear-resistant seamless steel pipe perforated plug. Example
[0043] (1) Preparation of seamless steel pipe perforated plug matrix: 0.34% pure carbon, 0.76% pure silicon, 0.41% metal manganese, 2.06% metal chromium, 0.48% metal vanadium, 2.79% metal nickel, 0.23% metal tungsten, 0.1% pure nitrogen, 0.15% lanthanum aluminum alloy, and the balance metal iron are added to a medium frequency induction furnace, heated to 1000°C and smelted for 3 h. After being completely melted, they are poured into a preheated stainless steel mold and vacuumed for vacuum casting. After molding, they are placed in a muffle furnace at 600°C and kept warm for 35 min to obtain a seamless steel pipe perforated plug matrix.
[0044] (2) Preparation of the seamless steel pipe perforated plug pre-finished product: The seamless steel pipe perforated plug substrate is placed in a muffle furnace, heated to 960°C at a rate of 6°C / min, quenched for 5 h, then cooled to 650°C at a rate of 8°C / min, tempered for 4 h, and air-cooled to obtain the seamless steel pipe perforated plug pre-finished product.
[0045] (3) Preparation of zirconium-chromium powder: Add 2 mmol of zirconium chloride and 20 mL of anhydrous ethanol to a reaction flask. After mixing evenly, add 2.7 mmol of chromium carbonate. React at 65°C for 10 h. Vacuum distillation is performed to obtain white sandy particles. The particles are then calcined at 800°C for 2 h and cooled to room temperature to obtain zirconium-chromium powder.
[0046] (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the pre-finished product of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The spraying power is 35 kW, the working voltage is 60 V, and the working current is 480 A. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. Argon gas is used to send zirconium-chromium powder from the nozzle into the plasma jet at a flow rate of 310 L / h and a speed of 6 g / min. It is heated to a molten state and sprayed onto the surface of the pre-finished product of the seamless steel pipe perforated plug to form a zirconium-chromium coating with a thickness of 1 mm to obtain a wear-resistant seamless steel pipe perforated plug.
[0047] Comparative Example 1
[0048] The difference between this comparative example and Example 1 is that no molten steel purifier is added in step (1), and other conditions remain the same.
[0049] Table 1 Elements and contents of seamless steel pipe perforation plug
[0050]
[0051] Vickers hardness test: A microhardness tester is used to measure the Vickers hardness of the perforated head of the seamless steel pipe. The measuring points are located on the coating surface, substrate, and the interface between substrate and coating. The indenter load used is 0.98N and the indenter time is 20s.
[0052] Table 2 Vickers hardness test
[0053]
[0054] From the test results in the above table, it can be seen that with the increase of the content of molten steel purifier, the Vickers hardness of the perforated head of the seamless steel pipe gradually increases. This is because the rare earth elements in the molten steel purifier react with O and S in the molten steel to generate rare earth oxides, rare earth sulfur oxides and rare earth sulfide inclusions, reducing the O and S content in the molten steel. The dispersed small spherical rare earth sulfide inclusions can replace the long strips of MnS inclusions in the steel, improving the toughness and hardness of the molten steel. At the same time, the deoxidation ability of magnesium and aluminum is significantly stronger than the desulfurization ability. The synergistic treatment of magnesium-cerium alloy can change the type of inclusions in the molten steel and reduce the inclusions. The ability of aggregation and floating can improve the purity of molten steel, and then precipitate fine and dispersed high-melting point compounds before the molten steel solidifies, reduce the supercooling of the molten steel, refine the grains after the molten steel solidifies, and improve the strength of the piercing plug; in addition, the radius of rare earth elements is large and it is difficult to diffuse in the grains. The rare earth atoms concentrated at the grain boundaries can also pin the grain boundaries, thereby improving the hardness of the piercing plug; the Vickers hardness of the coating area in the above table data is significantly higher than that of the substrate area and the junction, indicating that spraying zirconium-chromium powder on the plug surface can improve the surface hardness of the piercing plug, thereby increasing the service life of the piercing plug. Example
[0055] The difference between this embodiment and embodiment 1 is that the thickness of the zirconium-chromium coating in step (4) is 2 mm, and other conditions remain the same. Example
[0056] The difference between this embodiment and embodiment 1 is that the thickness of the zirconium-chromium coating in step (4) is 3 mm, and other conditions remain the same. Example
[0057] The difference between this embodiment and embodiment 1 is that the thickness of the zirconium-chromium coating in step (4) is 4 mm, and other conditions remain the same. Example
[0058] The difference between this embodiment and embodiment 1 is that the thickness of the zirconium-chromium coating in step (4) is 5 mm, and other conditions remain the same.
[0059] Comparative Example 2
[0060] The difference between this comparative example and Example 1 is that the zirconium-chromium coating spraying process is not performed, and other conditions remain the same.
[0061] Wear resistance test: The test was carried out using a ring-block friction tester. The grinding ring was quenched and low-temperature tempered 45# steel. The test conditions were a normal load of 98N, a test ring rotation speed of 400r / min, a wear time of 10h, and an analytical balance was used to weigh the sample wear.
[0062] Table 3 Wear and hardness test
[0063]
[0064] It can be seen from the test results in the above table that with the increase of the thickness of the zirconium-chromium coating, the wear amount of the perforated head of the seamless steel pipe gradually decreases. After 10 hours of wear, the wear amount of the perforated head in Example 9 is only 0.03g. In Comparative Example 2, no spray coating operation was performed, and its wear amount reached 1.02g, and the wear was relatively serious; this is because the prepared zirconium-chromium coating has zirconium and chromium with excellent wear resistance, which can be used as a hard phase. During the friction and wear process, it can effectively resist the wear of external abrasive particles. The crack source and crack propagation path of wear microcracks generated during wear are greatly restricted, and the sliding friction and chiseling of some abrasive particles on the coating surface can be converted into rolling, which reduces the wear of the coating by the abrasive particles, thereby improving the wear resistance of the perforated head of the seamless steel pipe.
[0065] High temperature resistance test: Referring to HB7236-95 standard, the seamless steel pipe perforated head specimen is heated to 800℃ in a box-type resistance furnace, taken out after keeping warm for 15 minutes, and quickly cooled to room temperature in cold water. After it is dried, it is repeated until the coating cracks or peels off. The high temperature resistance and thermal fatigue resistance of the coating are judged by the number of cycles it can withstand.
[0066] Table 4 High temperature resistance test
[0067]
[0068] It can be seen from the test data in the above table that with the increase of the thickness of the zirconium-chromium coating, the high temperature resistance of the seamless steel pipe perforation plug gradually increases. This is because the prepared zirconium-chromium coating is tightly bonded to the substrate and has a small amount of micro-area metallurgical bonding. The coating structure is relatively dense. Under high temperature, cracks are not easy to expand inward along the grain boundaries, avoiding premature failure of the perforation plug such as cracking and meat loss during use, thereby extending the service life of the perforation plug.
[0069] The above embodiments are only exemplary embodiments of the present invention and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present invention, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.
Claims
1. A method for preparing a wear-resistant seamless steel pipe perforation plug, characterized in that: The preparation method is carried out according to the following steps: (1) Preparation of seamless steel pipe perforated plug matrix: 0.28-0.42% by mass of pure carbon, 0.45-0.78% by mass of pure silicon, 0.31-0.52% by mass of metal manganese, 1.85-2.63% by mass of metal chromium, 0.33-0.54% by mass of metal vanadium, 2.23-2.89% by mass of metal nickel, 0.15-0.25% by mass of metal tungsten, 0.01-0.1% by mass of pure nitrogen, 0.03-0.15% by mass of steel liquid purifier, and the balance being metal iron, are added into a medium frequency induction furnace, heated for smelting, and after being completely melted, poured into a preheated stainless steel mold, vacuumed for vacuum casting, and placed in a muffle furnace at 500-650°C for 30-50 minutes to obtain a seamless steel pipe perforated plug matrix; The molten steel purifier is any one of magnesium-cerium alloy, rhenium-magnesium alloy or lanthanum-aluminum alloy; (2) Preparation of the seamless steel pipe perforated plug pre-finished product: placing the seamless steel pipe perforated plug substrate in a muffle furnace, heating it at a rate of 3-6°C / min for quenching, then cooling it at a rate of 6-10°C / min for tempering, and air cooling it after it is taken out of the furnace to obtain the seamless steel pipe perforated plug pre-finished product; (3) Preparation of zirconium-chromium powder: Add zirconium chloride and anhydrous ethanol to a reaction flask, mix well, add chromium carbonate, stir to react, and after the reaction is completed, vacuum distill to obtain white sandy particles, then calcine at 600-800°C for 1-3 hours, cool to room temperature, and obtain zirconium-chromium powder; (4) Preparation of wear-resistant seamless steel pipe perforated plugs: After the surface of the seamless steel pipe perforated plug is cleaned, derusted and roughened by sandblasting, it is sprayed with a plasma spray gun. The nozzle and electrode of the spray gun are respectively connected to the positive and negative poles of the power supply. Plasma gas is passed between the nozzle and the electrode. The arc is ignited by high-frequency sparks. The powder feeding gas feeds zirconium-chromium powder from the nozzle into the plasma jet, heats it to a molten state, and sprays it onto the surface of the seamless steel pipe perforated plug, forming a zirconium-chromium coating with a thickness of 1-5 mm to obtain a wear-resistant seamless steel pipe perforated plug.
2. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In the step (1), the smelting temperature is 950-1100° C. and the smelting time is 1-3 hours.
3. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In the step (2), the quenching temperature is 900-1050°C and the quenching time is 3-6h.
4. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In the step (2), the tempering temperature is 550-700° C. and the tempering time is 1-4 hours.
5. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In the step (3), the ratio of zirconium chloride to chromium carbonate is 1 mol: (1.1-1.4) mol.
6. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In the step (3), the reaction temperature is 60-70° C. and the reaction time is 5-10 h.
7. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In step (4), the powder feeding gas is any one of argon, hydrogen, helium and nitrogen.
8. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In the step (4), the plasma spray gun has a spraying power of 25-35 kW, an operating voltage of 55-65 V, and an operating current of 450-550 A.
9. The method for preparing a wear-resistant seamless steel pipe perforation plug according to claim 1, characterized in that: In step (4), the powder feeding gas flow rate is 280-320 L / h, and the powder feeding speed is 5-8 g / min.