Amino acid modified silica and preparation method thereof, resin mold and preparation method thereof

Through the combination of amino acid-modified silica and modified epoxy resin, the problem of balancing the porosity and flexural strength of the resin mold is solved, and the preparation of the resin mold with high porosity and good mechanical properties is achieved.

CN118047384BActive Publication Date: 2024-10-01BEIJING INST OF TECH TANGSHAN RES INST
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410048688.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-12
Publication Date
2024-10-01
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

While existing resin molds increase porosity, they suffer serious loss of flexural strength, making it difficult to achieve both high porosity and good mechanical properties.

Method used

By modifying the spherical silica with double bonds on the surface with amino acids, introducing carboxyl groups, and combining calcium carbonate and titanium dioxide to improve the porosity and mechanical properties of the resin mold, modified epoxy resin and water-based curing agent are used. Combined to form a resin mold with high porosity.

Benefits of technology

Significantly improves the porosity and mechanical properties of the resin mold, ensuring rapid diffusion and penetration of moisture while maintaining high bending strength and flexural strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an amino acid modified silica and a preparation method thereof and a resin mold and a preparation method thereof, and relates to the technical field of resin molds. The invention introduces a carboxyl group on the side group of spherical silica containing double bonds on the surface, improves hydrophilicity by modifying the carboxyl group, thereby greatly improving the porosity of the finished resin mold, and introduces calcium carbonate and titanium dioxide to obtain a good modification effect. Adding modified fillers can greatly improve the water absorption rate of the resin mold. The higher the water absorption rate, the more open holes, the more connected holes, the higher the porosity, and the mechanical properties of the mold can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of resin molds, and in particular to amino acid-modified silica and a preparation method thereof, and a resin mold and a preparation method thereof. Background Art

[0002] High-pressure grouting is a type of pressure grouting forming process, which is mainly used in the production process of various large-scale ceramic sanitary ware. From the perspective of specific operation properties, high-pressure grouting belongs to the filter pressing process, which relies on applying sufficient pressure to the mold to dialyze the liquid. Therefore, the mold is required to have good filtration properties. At present, sanitary ceramic products choose porous resin molds. In the process of making sanitary ceramics, production personnel apply pressure to the mud to allow water to quickly diffuse, penetrate, penetrate and be removed from the model to obtain a blank with good thickness and ideal strength. The material and porosity of the mold become the key to determining the thickness and strength of the blank in this process.

[0003] Publication No. CN115678209A discloses a resin composition for manufacturing a high-pressure mold and a method of using the same, comprising epoxy resin, dispersant, silica sand powder, alumina, curing agent and water. By mixing these components, the resin mold can be used at room temperature. The porosity of the resin mold is increased, but as the porosity increases, its flexural strength is severely lost. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an amino acid modified silica and a preparation method thereof, and a resin mold and a preparation method thereof, so as to improve the porosity of the resin mold.

[0005] In the first aspect, the present invention proposes a method for preparing amino acid-modified silica, in which spherical silica containing double bonds on the surface is side-group modified, and highly hydrophilic carboxyl groups are introduced into the side chains of silica through a hydrosilylation reaction, thereby improving the porosity of the finished resin mold.

[0006] The preparation method of modified silicon dioxide comprises the following steps:

[0007] Adding silica balls with double bonds on the surface, N-acetyl-L-cysteine, photocatalyst 2,2-dihydroxymethylpropionic acid and tetrahydrofuran into the reactor in sequence, and stirring to disperse them uniformly;

[0008] Then, the mixture was stirred and irradiated with an ultraviolet lamp having a main wavelength of 365 nm to react. After the reaction was completed, tetrahydrofuran was removed in vacuo to obtain a primary product.

[0009] The primary product is precipitated in methanol three times to remove unreacted mercapto compounds and catalysts, and then vacuum dried to constant weight to obtain modified silica with carboxyl groups.

[0010] In the second aspect, amino acid-modified silica is obtained by the above method.

[0011] In a third aspect, the present invention provides a resin mold having a high porosity, which allows moisture to quickly diffuse, penetrate, penetrate and be removed from the mold, thereby obtaining a blank having a good thickness and an ideal strength.

[0012] The resin mold comprises a first component and a second component, measured by weight, wherein the first component comprises 20 to 30 parts of amino acid-modified silica obtained by the above method, 5 to 10 parts of calcium carbonate, 2 to 5 parts of titanium dioxide, 20 parts of crystalline silica, and 5 parts of an aqueous solution of an emulsifier; the second component comprises 30 parts of a modified epoxy resin and 6 to 8 parts of an aqueous curing agent, wherein the modified epoxy resin is a mixture of E-51 epoxy resin and LSC-206 epoxy resin.

[0013] Furthermore, the emulsifier is OP-10 emulsifier, and the mass concentration of the emulsifier aqueous solution is 10wt%.

[0014] In a fourth aspect, the present invention provides a method for preparing a resin mold, by adding modified silica to improve the porosity and mechanical properties of the resin mold.

[0015] The method for preparing a resin mold comprises the following steps:

[0016] S1. Add distilled water to the first stirring barrel, add calcium carbonate and titanium dioxide to the amino acid-modified silica and add the mixture to the first stirring barrel and continue stirring for 12 hours, then add crystalline silica and OP-10 emulsifier aqueous solution to the mixture, continue stirring until fully mixed, and obtain the first component;

[0017] S2, adding LSC-206 resin to E-51 epoxy resin and stirring to obtain modified epoxy resin;

[0018] The modified epoxy resin and the water-based curing agent are mixed and stirred until fully mixed to obtain a uniform light yellow viscous liquid, thereby obtaining a second component;

[0019] S3. Under stirring conditions, add the second component to the first component, mix evenly, and obtain a uniform white viscous liquid. Place the white viscous liquid in a mold forming device, solidify it, and obtain a mold.

[0020] Furthermore, the emulsifier aqueous solution in S1 is an OP-10 aqueous solution with a mass concentration of 10%, and the mass ratio of distilled water, modified silica, calcium carbonate, titanium dioxide, crystalline silica and emulsifier aqueous solution is 23: (20-30): (5-10): (2-5): 20: 5.

[0021] Furthermore, the stirring speed in S1 is 180 rpm, the speed in S2 is 500 rpm, and the speed in S3 is 480 rpm.

[0022] Furthermore, in S2, the mass ratio of E-51 epoxy resin to LSC-206 resin is 18:12, and the mass ratio of modified epoxy resin to water-based curing agent is 30:(6~8).

[0023] Compared with the prior art, the present invention has at least the following beneficial effects: the present invention introduces carboxyl groups on the side groups of spherical silica containing double bonds on the surface, improves hydrophilicity by modifying the carboxyl groups, thereby greatly improving the porosity of the finished resin mold, and introduces calcium carbonate and titanium dioxide to achieve a good modification effect. Adding modified fillers can greatly improve the water absorption rate of the resin mold. The higher the water absorption rate, the more open holes, the more connected holes, the higher the porosity, and can improve the mechanical properties of the mold. DETAILED DESCRIPTION

[0024] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific implementation methods, but the present invention is not limited thereto.

[0025] The invention provides a preparation method of amino acid modified silica. A highly hydrophilic carboxyl group is introduced into a side chain of a silica ball containing double bonds on the surface by a hydrosilylation reaction, thereby enhancing the hydrophilicity of a resin mold and further improving the porosity of the mold. The steps are as follows: 1 g of silica balls containing double bonds on the surface (prepared by using the prior art), 2.5 g of N-acetyl-L-cysteine, 0.06 g of a photocatalyst 2,2-dihydroxymethylpropionic acid (DMPA) and 10 mL of tetrahydrofuran (THF) are sequentially added into a reactor, after the reactants are evenly dispersed, stirring is maintained at a speed of 180 rpm and irradiated under an ultraviolet lamp with a wavelength of 365 nm for reaction for 5 minutes, after the reaction is completed, THF is removed in vacuo, the reaction product is precipitated in methanol for three times to remove unreacted thiol compounds and catalysts, and the amino acid modified silica with carboxyl groups is obtained after vacuum drying to constant weight.

[0026] FT-IR ( KBr,cm -1 ): v=3594, 3346, 2963, 2905, 1733, 1662, 1408, 1259,1094, 1014, 866.

[0027] The amino acid modified silica was subjected to infrared testing, and the results are as above. Analysis of the infrared results shows that characteristic absorption peaks of functional groups such as carboxyl groups appear on the surface of the modified silica, which indicates that the reaction formula of the amino acid modified silica is as follows:

[0028]

[0029] The present invention introduces a carboxyl group into the side group of the silicon dioxide containing double bonds on the surface, so that the amino acid-modified silicon dioxide has slight acidity and enhances its hydrophilicity, thereby improving the porosity of the mold. Example 1

[0030] A method for preparing a resin mold, the steps are as follows:

[0031] S1. Add 23g of water into a stirring barrel, and add 25g of the amino acid-modified silica obtained by the above preparation method, 10g of calcium carbonate and 5g of titanium dioxide. After stirring at 32°C for 12h, add 20g of crystalline silica ZB3000 and an aqueous solution of emulsifier OP-10 (0.5g of OP-10 and 4.5g of water) and stir at 180 rpm until the components are fully mixed and the powder is free of caking to obtain the first component.

[0032] S2. Add 12 g of LSC-206 resin to 18 g of E-51 epoxy resin, stir at 32° C. for 12 h to obtain a modified epoxy resin; mix 30 g of the obtained modified epoxy resin, 3.36 g of a water-based curing agent (2801-FT) and 3 g of a water-based curing agent (502), and stir at a speed of 500 rpm until all components are fully mixed to obtain a uniform light yellow viscous liquid, thereby obtaining a second component.

[0033] S3. Under stirring conditions at a speed of 480 rpm, add the second component to the first component until the components are fully mixed to obtain a uniform white viscous liquid. Place the white viscous liquid in a mold forming device and cure it at 32°C for 12 hours to obtain a resin mold. Example 2

[0034] The preparation method is the same as that of Example 1, except that the amounts of the following ingredients are changed: 30 g of amino acid-modified silica, 10 g of calcium carbonate, 5 g of titanium dioxide, and 20 g of crystalline silica ZB3000. Example 3

[0035] The preparation method is the same as that of Example 1, except that the amounts of the following ingredients are changed: 20 g amino acid-modified silica, 5 g calcium carbonate, 2 g titanium dioxide, and 20 g crystalline silica ZB3000.

[0036] Comparative Example 1

[0037] The preparation method is the same as that of Example 1, except that the following ingredients are changed: 30 g of spherical silica containing double bonds on the surface, 10 g of calcium carbonate, 5 g of titanium dioxide, and 20 g of crystalline silica ZB3000.

[0038] Comparative Example 2

[0039] The preparation method is the same as that of Example 1, except that the following ingredients are changed: 15 g amino acid-modified silica, 10 g calcium carbonate, 5 g titanium dioxide, and 20 g crystalline silica ZB3000.

[0040] Comparative Example 3

[0041] The preparation method is the same as that of Example 1, except that the following ingredients are changed: 50 g amino acid modified silica, 10 g calcium carbonate, 5 g titanium dioxide, and 20 g crystalline silica ZB3000.

[0042] The bending strength, porosity and flexural strength of the resin molds obtained in Examples 1-3 and Comparative Examples 1-3 were tested respectively. The bending strength of the molds was tested according to GB / T 9341-2008 Bending Properties of Plastics. Different resin molds were made into rectangular test bars of the same size and the flexural strength was tested using a universal testing machine. The porosity was tested using a mercury intrusion instrument.

[0043] Bending strength (MPa) Porosity (%) Flexural strength (MPa) Example 1 9.32 40.78 9.32 Example 2 10.96 45.61 10.96 Example 3 10.33 47.88 10.33 Comparative Example 1 4.32 20.93 4.32 Comparative Example 2 3.55 32.07 3.55 Comparative Example 3 3.23 26.54 3.23

[0044] Compared with spherical silica containing double bonds on the surface as filler, the amino acid-modified silica used in the present invention can improve and maintain high bending strength while increasing the porosity of the mold.

[0045] Finally, it should be noted that the above are only preferred embodiments of the present invention. Of course, those skilled in the art can make changes and modifications to the present invention. If these modifications and variations fall within the scope of the claims of the present invention and their equivalent technologies, they should be considered to be within the scope of protection of the present invention.

Claims

1. A resin mold, characterized in that: The composition comprises a first component and a second component, wherein the first component comprises 20~30 parts of amino acid modified silica, 5-10 parts calcium carbonate, 2~5 parts of titanium dioxide, 20~30 parts of crystalline silicon dioxide, 5 parts of an aqueous solution of an emulsifier; The second component includes 30 parts of modified epoxy resin and 6-8 parts of water-based curing agent, and the modified epoxy resin is a mixture of E-51 epoxy resin and LSC-206 epoxy resin; The preparation method of the amino acid modified silicon dioxide comprises the following steps: Adding silica balls with double bonds on the surface, N-acetyl-L-cysteine, photocatalyst 2,2-dihydroxymethylpropionic acid and tetrahydrofuran into the reactor in sequence, and stirring to disperse them uniformly; Then, the mixture was stirred and irradiated with an ultraviolet lamp having a main wavelength of 365 nm to react. After the reaction was completed, tetrahydrofuran was removed in vacuo to obtain a primary product. The primary product is precipitated in methanol three times to remove unreacted thiol compounds and catalysts, and then vacuum dried to constant weight to obtain amino acid-modified silica with carboxyl groups.

2. The resin mold according to claim 1, characterized in that: The emulsifier is OP-10 emulsifier, and the mass concentration of the emulsifier aqueous solution is 10wt%.

3. A method for preparing a resin mold, characterized in that: The steps include: S1. Add distilled water to the first stirring barrel, add amino acid-modified silica, calcium carbonate and titanium dioxide to the first stirring barrel and continue stirring for 12 hours, then add crystalline silica and OP-10 emulsifier aqueous solution to the first stirring barrel, continue stirring until fully mixed, and obtain the first component; The preparation method of the amino acid modified silicon dioxide comprises the following steps: Adding silica balls with double bonds on the surface, N-acetyl-L-cysteine, photocatalyst 2,2-dihydroxymethylpropionic acid and tetrahydrofuran into the reactor in sequence, and stirring to disperse them uniformly; Then, the mixture was stirred and irradiated with an ultraviolet lamp having a main wavelength of 365 nm to react. After the reaction was completed, tetrahydrofuran was removed in vacuo to obtain a primary product. The primary product is precipitated in methanol three times to remove unreacted thiol compounds and catalysts, and then vacuum dried to constant weight to obtain amino acid-modified silica with carboxyl groups; S2, adding LSC-206 resin to E-51 epoxy resin and stirring to obtain modified epoxy resin; The modified epoxy resin and the water-based curing agent are mixed and stirred until fully mixed to obtain a uniform light yellow viscous liquid, thereby obtaining a second component; S3. Under stirring conditions, add the second component to the first component, mix evenly, and obtain a uniform white viscous liquid. Place the white viscous liquid in a mold forming device, solidify it, and obtain a mold.

4. The method for preparing a resin mold according to claim 3, characterized in that: The emulsifier aqueous solution in S1 is an OP-10 aqueous solution with a mass concentration of 10%, and the mass ratio of distilled water, amino acid-modified silica, calcium carbonate, titanium dioxide, crystalline silica and emulsifier aqueous solution is 23: (20~30): (5~10): (2~5): 20:

5.

5. The method for preparing a resin mold according to claim 3, characterized in that: The stirring speed in S1 was 180 rpm, in S2 it was 500 rpm, and in S3 it was 480 rpm.

6. The method for preparing a resin mold according to claim 3, characterized in that: The mass ratio of E-51 epoxy resin and LSC-206 resin in S2 is 18:12, and the mass ratio of modified epoxy resin and water-based curing agent is 30:(6~8).

Citation Information

Patent Citations

  • Resin composition for manufacturing high-pressure mold and use method thereof

    CN115678209A

  • Preparation method and application of surface-modified nano-silica

    CN104277191A

  • Waterborne epoxy porous resin composite material as well as preparation method and application thereof

    CN107868232A

  • Surface modified porous silica and method for manufacturing the same

    JP2003313024A

  • Nano-Silica Dispersion Having Amphiphilic Properties And A Double-Particle Structure And Its Production Method

    US20190046939A1