A method for reducing basket tooth marks in heterojunction batteries

By performing steps such as pre-cleaning, texturing and post-cleaning of the silicon wafer, combined with chemical agents and bubbling processes, a regular small-sized pyramid structure is formed, which solves the problem of tooth marks on the heterojunction battery basket, reduces production costs and improves efficiency. Battery efficiency.

CN118198185BActive Publication Date: 2024-10-11江苏新璟宏能源科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410290970.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-10-11
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

Heterojunction cells are prone to produce tooth marks during the wet basket preparation process, leading to battery degradation and increased production costs. Existing solutions are costly and have limited effectiveness.

Method used

Through the steps of pre-cleaning, texturing, post-cleaning, rounding and drying of the silicon wafer, control the temperature, time and liquid ratio, use potassium hydroxide, hydrogen peroxide, hydrochloric acid, hydrofluoric acid and other chemical agents, combined with drum The foaming process and surfactant adjust the viscosity and surface tension of the texturing liquid to form a regular small-sized pyramid structure and reduce the roughness and reflectivity of the silicon wafer surface.

Benefits of technology

It significantly reduces the proportion of basket tooth marks, improves the cleanliness of the silicon wafer surface and the uniformity of the pyramid structure, reduces production costs, and improves the conversion efficiency and production efficiency of heterojunction cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118198185B_ABST
    Figure CN118198185B_ABST
Patent Text Reader

Abstract

The present invention provides a method for reducing the basket tooth mark of a heterojunction battery. After the silicon wafer is textured, hydrogen peroxide is used as a strong oxidant to oxidize and dissolve the organic pollutants and damaged layers on the surface of the silicon wafer, thereby improving the cleanliness of the surface of the silicon wafer. When the hydrogen peroxide is excessive, potassium hydroxide will cause excessive corrosion of the silicon wafer, resulting in poor pyramid formation and high surface micro-roughness, which is particularly obvious in places where the gaps of the flower basket are blocked. The proportion of basket tooth marks is high. Therefore, the present application can reduce the micro-roughness of the velvet surface by mixing potassium hydroxide and hydrogen peroxide in a proportion and stabilizing the volume self-replenishing ratio at 1:2-1:3, thereby greatly reducing the proportion of basket tooth marks. The surface tension of the silicon wafer is reduced by setting the alkali and additives in the texture liquid, the wettability and fluidity of the texture liquid are improved, and the bubbling function is turned on at the same time. The surface of the silicon wafer presents a regular, small-sized, uniform, and dense pyramid velvet structure through the texture temperature, time, and process ratio, and the proportion of basket tooth marks is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heterojunction battery manufacturing, and in particular to a method for reducing basket tooth marks of heterojunction batteries. Background Art

[0002] Heterojunction cells are a type of high-efficiency photovoltaic solar cells. Compared with traditional crystalline silicon photovoltaic solar cells, heterojunction cells are increasingly favored by the market due to their higher conversion efficiency. Heterojunction cells are single-crystal N-type cells. First, they also need to go through trough texturing to prepare a pyramid-structured velvet surface. When using a wet flower basket, basket teeth marks will inevitably be produced. This is because the concentration of potassium silicate or sodium silicate accumulates in the texturing trough. Sodium silicate or potassium silicate is in a colloidal state in the solution, which greatly increases the viscosity of the solution and has a buffering effect on the transport process of hydroxide ions from the etching solution to the reaction interface.

[0003] When the content of sodium silicate and potassium silicate in the texturing solution is 2.5-30wt%, the solution has good selectivity, and a velvet surface completely covering the pyramids can be produced on the surface of the silicon wafer. As the content of sodium silicate or potassium silicate increases, the viscosity of the solution increases, and the fluidity is poor. The two sides of the silicon wafer are blocked by the gaps in the flower basket, resulting in insufficient texturing, poor velvet removal effect and cleaning effect. After preparing amorphous silicon film and transparent conductive film (TCO conductive film), the PN junction is destroyed, and there are defects under PL that appear as basket-tooth-shaped black spots, commonly known as basket-tooth marks, which cause heterojunction batteries to degrade, affect the yield and increase production costs. The traditional solution is to clean and soak the flower basket with alkali solution or improve the flower basket. After multiple experiments, the flower basket soaked in alkali solution did not improve the heterojunction basket tooth mark, and the flower basket improvement requires the replacement of the flower basket, which has a high cost investment. Therefore, it is necessary to develop a low-cost and effective process method to reduce the basket tooth mark. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a method for reducing basket marks of heterojunction cells, so as to solve the problem that basket marks will be generated on the surface of silicon wafers during wet basket forming in the prior art.

[0005] To achieve the above purposes and other related purposes,

[0006] The present invention provides a method for reducing tooth marks on heterojunction battery baskets, which comprises sequentially subjecting a basket carrying silicon wafers to the following steps:

[0007] S1, pre-cleaning the silicon wafer to remove particles and mechanical damage on the surface of the silicon wafer;

[0008] S2, a pyramid structure is formed on the surface of the silicon wafer by a texturing liquid, the temperature is controlled at 70-80℃, the time is 300-500s, and the weight loss is controlled at 0.3-0.35g / pcs;

[0009] S3, control the temperature to 60-70℃, the time to 90-100s, and control the weight loss to 0.02-0.05g / pcs through the secondary texturing liquid;

[0010] S4, post-cleaning the silicon wafer by preparing a tank with potassium hydroxide and hydrogen peroxide in a volume ratio of 1:110-130, controlling the temperature to 60-70°C, and the time to 240-300s, the potassium hydroxide is replenished according to the batch number, and the hydrogen peroxide is replenished according to the time, so that the volume ratio of potassium hydroxide and hydrogen peroxide is stabilized at 1:2-1:3;

[0011] S5, preparing a bath with hydrochloric acid and hydrofluoric acid in a volume ratio of 1:1.2-1:1.5, and simultaneously introducing 30-45ppm of ozone to round the surface of the silicon wafer, and controlling the rounding time to 60-80s and the temperature to 60-80°C;

[0012] S6, cleaning with a mixture of hydrochloric acid and hydrogen peroxide;

[0013] S7, using hydrofluoric acid to remove silicon dioxide on the surface of the silicon wafer and make the surface of the silicon wafer hydrophobic;

[0014] S8, drying the silicon wafer and the flower basket after slow pulling;

[0015] At least one pure water rinse is included between adjacent steps.

[0016] In one embodiment of the present invention, the liquids in S1-S8 are all in overflow state and assisted by bubbling process, and the primary texturing liquid has a concentration of 3-5% potassium hydroxide and 0.1-1.5% texturing additive;

[0017] The secondary texturing liquid contains 2-4% sodium hydroxide and 0.05-1% texturing additive.

[0018] In one embodiment of the present invention, the texturing additive includes a texturing catalyst, a surfactant and a suede modifier.

[0019] In one embodiment of the present invention, the texturing additive is composed of 0.01-0.1 wt % of a texturing catalyst, 1-2 wt % of a surfactant, 1.5-2.5 wt % of a suede modifier, and the remaining components are pure water.

[0020] In one embodiment of the present invention, the surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and sodium alkylnaphthalene sulfonate.

[0021] In one embodiment of the present invention, the suede finishing agent is one or more of hydroxy-β-cyclodextrin, amino-β-cyclodextrin or methyl-β-cyclodextrin.

[0022] In one embodiment of the present invention, the texturing catalyst is sodium lignin sulfonate or sodium dodecyl diphenyl ether sulfonate.

[0023] In one embodiment of the present invention, the pre-cleaning in S1 includes the following steps:

[0024] Step 1, using ultrasound and 5-8% sodium hydroxide or potassium hydroxide, controlling the temperature at 60-80° C. for 100-200 seconds to remove particles on the surface of the silicon wafer;

[0025] Step 2, using 3-5% hydrofluoric acid and 0.2-0.5% hydrochloric acid at a temperature of 40-60° C. for 80-160 seconds to remove the oxide layer on the surface of the silicon wafer;

[0026] Step 3, using potassium hydroxide with a concentration of 6-8%, controlling the temperature to 50-70° C., and the time to 100-150 seconds to remove mechanical damage on the surface of the silicon wafer;

[0027] Step 4, pre-cleaning the silicon wafer with a mixture of 4-6% hydrogen peroxide and 4-6% potassium hydroxide;

[0028] At least one pure water rinse is included between adjacent steps.

[0029] In one embodiment of the present invention, the hydrochloric acid and the hydrogen peroxide in S6 are prepared in a tank according to a volume ratio of 1:3-1:5; and the concentration of the hydrofluoric acid in S7 is 4-6%.

[0030] In one embodiment of the present invention, the temperature of the slow pulling in S8 is 60-70° C., and the time is 200-300 seconds.

[0031] As described above, a method for reducing basket tooth marks of heterojunction batteries of the present invention has the following beneficial effects:

[0032] 1. S4 is the first cleaning step after texturing. Hydrogen peroxide is used as a strong oxidant to oxidize and dissolve organic pollutants and damaged layers on the surface of the silicon wafer to improve the cleanliness of the silicon wafer surface. When there is an excess of hydrogen peroxide, potassium hydroxide will over-corrode the silicon wafer, resulting in poor pyramid formation and high surface micro-roughness, which is particularly obvious in places where the flower basket gaps are blocked. The proportion of basket teeth marks is high. Therefore, the present application reduces the micro-roughness of the suede surface by mixing potassium hydroxide and hydrogen peroxide in a proportional manner and stabilizing the volume self-complementing ratio at 1:2-1:3, thereby greatly reducing the proportion of basket teeth marks.

[0033] 2. The reason for the basket tooth mark of the battery may be that the texturing liquid is not wet enough. By setting the alkali and additives in the texturing liquid, the surface tension of the texturing liquid can be reduced, the wettability and fluidity of the texturing liquid can be improved, and the bubbling function can be turned on at the same time to reduce the contact area between the silicon wafer and the gap of the flower basket.

[0034] 3. In heterojunction cells, both pre-cleaning and texturing are cleaning treatments of silicon wafers by wet chemical methods. After the first texturing, a velvet surface with more microstructures is obtained, and the reflectivity of the silicon wafer is greatly reduced. The reflectivity is further reduced by improving the appearance of the velvet surface through the second texturing. The texturing temperature is a key factor affecting the diffusion of texturing additives, hydroxide, hydrogen bubbles, and silicate product ions in the solution. This application improves the texturing effect by setting the texturing temperature at a reasonable temperature.

[0035] 4. The present application introduces sulfonic acid groups and hydroxyl groups into the texturing catalyst, which can effectively regulate the adsorption strength of the auxiliary molecules and silicon and ensure the high water solubility of the auxiliary molecules, thereby achieving fine control of the silicon surface structure. The surfactant can reduce the surface tension of the texturing liquid so that the bubbles can quickly detach from the silicon wafer surface. The bubble size is small when leaving, and the size of the resulting pyramid is correspondingly smaller and the number of nucleation points increases, which significantly increases the number of pyramids. The increase of surfactants can improve the degassing effect of silicon wafers and reduce the watermarks produced on the silicon surface. The surface of the silicon wafer presents a regular, small-sized, uniform, and dense pyramid velvet structure through the texturing temperature, time, and process ratio.

[0036] 5. In order to prevent the tip of the pyramid from being too sharp after the silicon wafer is texturized, which may cause cracks in the amorphous silicon film and cause leakage during the subsequent amorphous silicon film deposition process, a rounding process is added. By adjusting the acid ratio and the rounding time, the silicon wafer can obtain a more ideal carrier lifetime.

[0037] 6. The primary texturing mainly realizes the rapid growth of pyramids through higher concentration of chemical solution, and the secondary texturing adopts lower reaction concentration and shorter reaction time to achieve full corrosion effect, modify the pyramid morphology, and complete the later growth process of the velvet surface. The texturing reaction time in this application is also precisely controlled. The bubbling setting can improve the uniformity of the solution, the transport speed of the reactants, and the desorption effect of the bubbles. The overflow setting can ensure the concentration of the silicon wafer reaction solution. Potassium hydroxide and sodium hydroxide are used as the main solutions for texturing to etch the surface of the silicon wafer. The setting of the texturing additive can control the reaction speed, reduce the surface tension of the texturing solution, promote the reaction, and make the pyramids more uniform. The diameter and density of the bubbles have an important influence on the velvet surface structure and the corrosion rate. The texturing additive in this application is used to adjust the viscosity of the texturing solution to reduce the basket tooth mark. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Shown is the appearance of a basket tooth print.

[0039] Figure 2 Shown is the PL image of the basket tooth mark after using this method.

[0040] Figure 3 Shown is a comparison diagram of the basket tooth marks before and after the implementation of the present invention. DETAILED DESCRIPTION

[0041] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.

[0042] like Figures 1 to 3 As shown, a method for reducing tooth marks in heterojunction battery baskets is provided, wherein a basket carrying silicon wafers is sequentially subjected to the following steps: S1, pre-cleaning the silicon wafers to remove particles and mechanical damage on the surface of the silicon wafers; S2, forming a pyramid structure on the surface of the silicon wafers by a primary texturing liquid, controlling the temperature to 70-80°C, the time to 300-500s, and controlling the weight loss to 0.3-0.35g / pcs; S3, controlling the temperature to 60-70°C, the time to 90-100s, and controlling the weight loss to 0.02-0.05g / pcs by a secondary texturing liquid; S4, preparing a tank by mixing potassium hydroxide and hydrogen peroxide in a volume ratio of 1:110-130, controlling the temperature to 60-70°C, the time to 24 The silicon wafer is post-cleaned from 0 to 300 seconds, potassium hydroxide is replenished according to the batch number, and hydrogen peroxide is replenished according to the time, so that the volume ratio of potassium hydroxide and hydrogen peroxide is stabilized at 1:2-1:3; S5, hydrochloric acid and hydrofluoric acid are prepared in a tank at a volume ratio of 1:1.2-1:1.5, and 30-45ppm of ozone is introduced to round the surface of the silicon wafer, and the rounding time is controlled to be 60-80 seconds, and the temperature is 60-80°C; S6, a mixed solution of hydrochloric acid and hydrogen peroxide is used for cleaning; S7, hydrofluoric acid is used to remove silicon dioxide on the surface of the silicon wafer, and the surface of the silicon wafer is made hydrophobic; S8, the silicon wafer and the flower basket are dried after slow pulling; at least one pure water cleaning is included between adjacent steps.

[0043] S4 is the first cleaning step after texturing. Hydrogen peroxide is used as a strong oxidant to oxidize and dissolve organic pollutants and damaged layers on the surface of the silicon wafer to improve the cleanliness of the silicon wafer surface. When there is an excess of hydrogen peroxide, potassium hydroxide will over-corrode the silicon wafer, resulting in poor pyramid formation and high surface micro-roughness, which is particularly obvious in places where the flower basket gaps are blocked. The proportion of basket-tooth marks is high. Therefore, the present application reduces the micro-roughness of the suede surface by mixing potassium hydroxide and hydrogen peroxide in a certain proportion and stabilizing the volume self-replenishing ratio at 1:2-1:3, thereby greatly reducing the proportion of basket-tooth marks.

[0044] In heterojunction cells, pre-cleaning and texturing are both cleaning processes for silicon wafers using wet chemical methods. After one texturing process, a velvet surface with more microstructures is obtained, and the reflectivity of the silicon wafer is greatly reduced. The reflectivity is further reduced by improving the appearance of the velvet surface through a secondary texturing process.

[0045] S5 is a rounding treatment. In order to avoid the pyramid tip being too sharp after the silicon wafer is textured, which may cause cracks in the amorphous silicon film and cause leakage during the subsequent amorphous silicon film deposition process, a rounding process is added. By adjusting the acid ratio and the rounding time, the silicon wafer can obtain a more ideal carrier lifetime.

[0046] The liquids in S1-S8 are all in overflow state and assisted by bubbling process. The concentration of the primary texturing liquid is 3-5% potassium hydroxide and 0.1-1.5% texturing additive; the concentration of the secondary texturing liquid is 2-4% sodium hydroxide and 0.05-1% texturing additive.

[0047] The reason for the battery's basket teeth mark may be that the wetting of the texturing liquid is not enough. By setting the alkali and additives in the texturing liquid, the surface tension of the silicon wafer is reduced, the wetting and fluidity of the texturing liquid are improved, and the bubbling function is turned on to reduce the area of ​​the silicon wafer blocked by the gaps in the flower basket. The texturing temperature is a key factor affecting the diffusion of texturing additives, hydroxide, hydrogen bubbles and silicate product ions in the solution. This application improves the texturing effect by setting the texturing temperature at a reasonable temperature.

[0048] The primary texturing mainly realizes the rapid growth of pyramids through a higher concentration of liquid medicine, and the secondary texturing adopts a lower reaction concentration and a shorter reaction time to achieve a full corrosion effect, modify the pyramid morphology, and complete the later growth process of the velvet. The texturing reaction time in this application is also precisely controlled. If the time is too short, the pyramid may not be formed yet, the surface coverage is insufficient, and if the time is too long, overlap occurs, the edges and corners disappear, and the reflectivity of the silicon wafer is finally affected. The bubbling setting can improve the uniformity of the solution, the transport speed of the reactants, and the desorption effect of the bubbles. The overflow setting can ensure the concentration of the silicon wafer reaction solution. Potassium hydroxide and sodium hydroxide are used as the main solutions for texturing to etch the surface of the silicon wafer. The setting of the texturing additive can control the reaction speed, reduce the surface tension of the texturing liquid, promote the reaction, and make the pyramid more uniform. The diameter and density of the bubbles have an important influence on the velvet structure and the corrosion rate, so the viscosity characteristics of the texturing liquid are adjusted by the texturing additive.

[0049] The texturing additives include texturing catalysts, surfactants, and texturing modifiers. In the early days, small molecule organic alcohols such as ethanol, isopropanol, and tert-butanol, and organic bases such as diamine, tetramethylammonium hydroxide, and ammonium fluoride were introduced into potassium hydroxide or sodium hydroxide texturing solutions as different additives to obtain certain texturing adjustment effects. Isopropanol was first put into early industrial applications, but it has the inherent defects of large and uneven pyramids on the surface of single crystal silicon, poor repeatability, and difficulty in significantly reducing light reflectivity; low boiling point, high volatility, and changes in system concentration that easily lead to unstable batch production; large dosage, toxicity, and high post-treatment costs for waste liquid and waste gas pollution. The additives in this application use an efficient and stable formula to effectively control the chemical reactions of different crystalline silicon atoms with hydroxide to prepare small and uniform low-reflectivity pyramid structures.

[0050] The texturing additive comprises 0.01-0.1 wt% of a texturing catalyst, 1-2 wt% of a surfactant, 1.5-2.5 wt% of a suede modifier, and the remaining components are pure water.

[0051] The surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and sodium alkylnaphthalene sulfonate. The suede finishing agent is one or more of hydroxy-β-cyclodextrin, amino-β-cyclodextrin, or methyl-β-cyclodextrin. The suede making catalyst is sodium lignin sulfonate or sodium dodecyl diphenyl ether sulfonate.

[0052] The present application introduces sulfonic acid groups and hydroxyl groups into the texturing catalyst, which can effectively regulate the adsorption strength of the auxiliary molecules and silicon and ensure the high water solubility of the auxiliary molecules, thereby achieving fine control of the silicon surface structure. The surfactant can reduce the surface tension of the texturing liquid so that the bubbles can quickly detach from the silicon wafer surface. The bubble size is small when leaving, and the size of the resulting pyramid is correspondingly smaller and the number of nucleation points increases, which significantly increases the number of pyramids. The increase of surfactants can improve the degassing effect of silicon wafers and reduce the watermarks produced on the silicon surface. Through the texturing temperature, time and process ratio, the surface of the silicon wafer presents a regular, small-sized, uniform and dense pyramid velvet structure.

[0053] The pre-cleaning in S1 includes the following steps: step 1, using ultrasound and 5-8% sodium hydroxide or potassium hydroxide, controlling the temperature at 60-80°C, and the time for 100-200s to remove particles on the surface of the silicon wafer; step 2, using 3-5% hydrofluoric acid and 0.2-0.5% hydrochloric acid, controlling the temperature at 40-60°C, and the time for 80-160s to remove the oxide layer on the surface of the silicon wafer; step 3, using 6-8% potassium hydroxide, controlling the temperature at 50-70°C, and the time for 100-150s to remove mechanical damage on the surface of the silicon wafer; step 4, using a mixed solution of 4-6% hydrogen peroxide and 4-6% potassium hydroxide to pre-clean the silicon wafer; at least one pure water cleaning is included between adjacent steps.

[0054] In step 1, ultrasound with a frequency of 700-1000KHZ is used, which will not form large hollow bubbles, thereby reducing the degree of damage to the surface of the silicon wafer. The ultrasonic pressure wave impacts the silicon wafer, has the ability to remove particles, and improves the cleaning ability of the cleaning solution. Pre-cleaning removes metal ions in the silicon wafer, reduces carrier recombination centers, and eliminates the hanging parts of each atom in the silicon wafer to the maximum extent, thereby improving the cleanliness of the silicon wafer surface.

[0055] The hydrochloric acid and hydrogen peroxide in S6 are prepared in a tank according to a volume ratio of 1:3-1:5; the concentration of hydrofluoric acid in S7 is 4-6%; the temperature of the slow pulling in S8 is 60-70°C and the time is 200-300S.

[0056] The slow pull in S8 is a drying system designed based on the surface tension and capillary action of water, also known as full pull. This technology is to immerse the silicon wafers in the flower basket into hot deionized water to clean the silicon wafers. After cleaning, the silicon wafers are slowly lifted from the water tank at a controlled speed. Because the silicon wafers are pulled up slowly and steadily, the water interface on the surface of the silicon wafer will not be interrupted, and the liquid will not form small water droplets. With the help of capillary action and surface tension, the surface of the silicon wafer will naturally become a dry surface.

[0057] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. All equivalent modifications or changes made by those skilled in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A method for reducing basket tooth marks of heterojunction batteries, characterized in that: The flower basket containing the silicon wafers is sequentially subjected to the following steps: S1, pre-cleaning the silicon wafer to remove particles and mechanical damage on the surface of the silicon wafer; S2, forming a pyramid structure on the surface of the silicon wafer through a texturing liquid, controlling the temperature to 70-80℃, the time to 300-500s, and controlling the weight loss to 0.3-0.35g / pcs; S3, control the temperature to 60-70℃, the time to 90-100s, and control the weight loss to 0.02-0.05g / pcs through the secondary texturing liquid; S4, post-cleaning the silicon wafer by preparing a tank with potassium hydroxide and hydrogen peroxide in a volume ratio of 1:110-130, controlling the temperature to 60-70°C, and the time to 240-300s, the potassium hydroxide is replenished according to the batch number, and the hydrogen peroxide is replenished according to the time, so that the volume ratio of potassium hydroxide and hydrogen peroxide is stabilized at 1:2-1:3; S5, preparing a bath with hydrochloric acid and hydrofluoric acid in a volume ratio of 1:1.2-1:1.5, and simultaneously introducing 30-45ppm of ozone to round the surface of the silicon wafer, and controlling the rounding time to 60-80s and the temperature to 60-80°C; S6, cleaning with a mixture of hydrochloric acid and hydrogen peroxide; S7, using hydrofluoric acid to remove silicon dioxide on the surface of the silicon wafer and make the surface of the silicon wafer hydrophobic; S8, drying the silicon wafer and the flower basket after slow pulling; At least one pure water wash is included between adjacent steps; The liquids in S1-S8 are all in overflow state and assisted by bubbling process, and the primary texturing liquid has a concentration of 3-5% potassium hydroxide and 0.1-1.5% texturing additive; The secondary texturing liquid contains 2-4% sodium hydroxide and 0.05-1% texturing additive.

2. A method for reducing basket tooth marks of heterojunction batteries according to claim 1, characterized in that: The texturing additives include a texturing catalyst, a surfactant and a suede surface modifier.

3. A method for reducing basket tooth marks of heterojunction batteries according to claim 2, characterized in that: The texturing additive comprises 0.01-0.1 wt% of a texturing catalyst, 1-2 wt% of a surfactant, 1.5-2.5 wt% of a suede modifier, and the remaining components are pure water.

4. A method for reducing basket tooth marks of heterojunction batteries according to claim 2, characterized in that: The surfactant is one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, and sodium alkylnaphthalene sulfonate.

5. The method for reducing basket tooth marks of heterojunction batteries according to claim 2, characterized in that: The suede modifying agent is one or more of hydroxy-β-cyclodextrin, amino-β-cyclodextrin or methyl-β-cyclodextrin.

6. A method for reducing basket tooth marks of heterojunction batteries according to claim 2, characterized in that: The texturing catalyst is sodium lignin sulfonate or sodium dodecyl diphenyl ether sulfonate.

7. The method for reducing basket tooth marks of heterojunction batteries according to claim 1, characterized in that: The pre-cleaning in S1 comprises the following steps: Step 1, using ultrasound and 5-8% sodium hydroxide or potassium hydroxide, controlling the temperature at 60-80° C. for 100-200 seconds to remove particles on the surface of the silicon wafer; Step 2, using 3-5% hydrofluoric acid and 0.2-0.5% hydrochloric acid at a temperature of 40-60° C. for 80-160 seconds to remove the oxide layer on the surface of the silicon wafer; Step 3, using potassium hydroxide with a concentration of 6-8%, controlling the temperature to 50-70° C., and the time to 100-150 seconds to remove mechanical damage on the surface of the silicon wafer; Step 4, pre-cleaning the silicon wafer with a mixture of 4-6% hydrogen peroxide and 4-6% potassium hydroxide; At least one pure water rinse is included between adjacent steps.

8. The method for reducing basket tooth marks of heterojunction batteries according to claim 1, characterized in that: The hydrochloric acid and hydrogen peroxide in the S6 are prepared in a tank according to a volume ratio of 1:3-1:5; the concentration of the hydrofluoric acid in the S7 is 4-6%.

9. The method for reducing basket tooth marks of heterojunction batteries according to claim 1, characterized in that: The temperature of the slow pulling in S8 is 60-70° C., and the time is 200-300 seconds.