A high-strength and high-damping gradient Al-Zn-Mg alloy and its preparation method and application
By regulating the content of Zn alloy and using the belt-sliding + extrusion composite process, the gradient structure of Al-Zn-Mg alloy was prepared, which solved the problem of insufficient strength and damping performance of traditional alloys, and achieved a coordinated improvement of high strength and high damping performance. , broadening its application prospects.
Patent Information
- Application Number
- CN202410320575.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-03-20
AI Technical Summary
Traditional Al-Zn-Mg alloys have high strength but poor damping performance, while high zinc Al-Zn-Mg alloys have excellent damping performance but low strength. The existing methods will reduce the toughness and strength of the alloy by adding a coarse second phase to improve the damping performance. And there is a lot of room for improvement in mechanical properties.
By regulating the content of Zn alloy, a gradient structure Al-Zn-Mg alloy is prepared by using the belt-shrinking + extrusion composite process. The core is low zinc, the intermediate layer is medium zinc, and the surface is high zinc, forming a typical deformation structure, double-dimensional The peak grain structure and recrystallized grain structure were combined with thermal extrusion method to prepare a high-strength high-damping gradient alloy.
It has achieved a coordinated improvement of high strength and excellent damping performance, broadening its application prospects in the fields of national defense and military industry, aerospace and other fields.
Smart Images

Figure CN118222894B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of high-strength and high-damping gradient alloys, and in particular relates to a high-strength and high-damping gradient Al-Zn-Mg alloy and a preparation method and application thereof. Background Art
[0002] Traditional Al-Zn-Mg alloys have high strength but poor damping performance (internal friction value <0.01), which limits their application in aviation parts requiring high damping; high-zinc Al-Zn-Mg alloys have excellent damping performance (internal friction value ≥0.02), but low strength (usually less than 400MPa). At present, the mainstream method to improve damping performance is to add coarse second phases to traditional Al-Zn-Mg alloys to improve their damping performance, such as: SiC, graphite, etc. However, the introduction of coarse second phases is bound to reduce the toughness and even strength of the alloy. The inventors previously prepared Al-Zn-Mg-Cu-Zr alloys with higher strength and high damping by regulating the Zn / Mg ratio in the alloy, but the mechanical properties of this alloy still have a lot of room for improvement. Summary of the invention
[0003] In view of the problems existing in the above-mentioned prior art, the present invention proposes a high-strength and high-damping gradient Al-Zn-Mg alloy and its preparation method and application. The present invention prepares a gradient structure Al-Zn-Mg alloy by regulating the Zn alloy and combining the strip spinning + extrusion composite process, thereby obtaining excellent mechanical properties and damping properties, thereby broadening its industrial application.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A high-strength and high-damping gradient Al-Zn-Mg alloy is composed of a core of a low-zinc Al-Zn-Mg alloy, an intermediate layer of a medium-zinc Al-Zn-Mg alloy, and a surface of a high-zinc Al-Zn-Mg alloy. The core structure is a typical deformation structure, the intermediate layer is a double-peak grain structure composed of equiaxed crystals and deformed grains, and the surface is a recrystallized grain composed of equiaxed crystals. This composite structure can obtain strong strength and excellent damping performance.
[0006] Furthermore, the Zn content in the low-zinc Al-Zn-Mg alloy is 4-8wt%; the Zn content in the medium-zinc Al-Zn-Mg alloy is 10-18wt%; and the Zn content in the high-zinc Al-Zn-Mg alloy is 20-45wt%.
[0007] The present invention also provides a method for preparing the high-strength and high-damping gradient Al-Zn-Mg alloy, comprising the following steps:
[0008] The low-zinc Al-Zn-Mg alloy strip blank, the medium-zinc Al-Zn-Mg alloy strip blank and the high-zinc Al-Zn-Mg alloy strip blank are prepared by melt spinning method;
[0009] A rod-shaped blank is prepared by a winding method, wherein the core of the rod-shaped blank is a low-zinc Al-Zn-Mg alloy strip blank, the middle layer is a medium-zinc Al-Zn-Mg alloy strip blank, and the surface is a high-zinc Al-Zn-Mg alloy strip blank;
[0010] The rod-shaped billet is made into an extruded billet by a hot isotropic extrusion method; then the extruded billet is homogenized and hot extruded to obtain a high-strength and high-damping gradient Al-Zn-Mg alloy.
[0011] Furthermore, the parameters of the hot extrusion method are: temperature 150-250°C, pressure 200-400MPa, and holding time 10-40min.
[0012] Furthermore, the homogenization refers to keeping the temperature at 350-420° C. for 0.5-2 h.
[0013] Furthermore, the parameters of the hot extrusion are: temperature 350-420°C, pressure 400-600t, and extrusion ratio 10-50.
[0014] The present invention also provides an application of the high-strength and high-damping gradient Al-Zn-Mg alloy in the preparation of national defense, military industry, and aerospace components.
[0015] Compared with the prior art, the present invention has the following advantages and technical effects:
[0016] The invention provides a high-strength and high-damping gradient Al-Zn-Mg alloy, wherein the surface of the alloy is a high-zinc Al-Zn-Mg alloy, the core is a low-zinc 7XXX series Al-Zn-Mg alloy, the middle layer is a medium-zinc Al-Zn-Mg alloy, and the Zn content decreases from 20-45wt% to 4-8wt% in the core from the surface to the core; the gradient alloy presents three different forms of organizational structures, namely: the surface is fine equiaxed crystals, the core is a deformed structure, and the organizational structure (middle layer structure) between the surface and the core is a typical bimodal grain structure; the deformed structure of the core of the gradient Al-Zn-Mg alloy has high strength, and the bimodal grain structure of the surface fine crystals and the middle layer has high damping and toughness, so the gradient Al-Zn-Mg alloy has high strength, toughness and damping performance; the high-strength and high-damping alloy has broad application prospects in the fields of national defense, military industry, aerospace, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0018] Figure 1 Schematic diagram of preparation of high-strength and high-damping gradient Al-Zn-Mg alloy in the present invention;
[0019] Figure 2 A schematic diagram of the longitudinal section metallographic structure of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention;
[0020] Figure 3 EBSD grayscale image of the surface equiaxed crystal of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention;
[0021] Figure 4 This is an EBSD grayscale image of the core deformation structure of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention;
[0022] Figure 5 This is an EBSD grayscale image of the bimodal grain structure of the middle layer of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0024] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0025] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0026] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0027] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0028] The "room temperature" mentioned in the present invention is 25±2°C unless otherwise specified.
[0029] The fine equiaxed crystals and bimodal grain structure have high toughness and excellent damping performance, and the deformed structure has high tensile strength. The recrystallization temperature of Al-Zn-Mg alloy is related to the Zn content. Generally, the higher the Zn content, the lower the recrystallization temperature, and recrystallization is easy to occur during hot extrusion, so the high-zinc Al-Zn-Mg alloy is easy to obtain a fine equiaxed crystal structure. In comparison, the traditional low-zinc Al-Zn-Mg alloy has a high recrystallization temperature, and it is easy to obtain a deformed structure during hot extrusion deformation, so it has high strength but low damping performance. The medium-zinc Al-Zn-Mg alloy undergoes partial dynamic recrystallization during hot extrusion to obtain a bimodal grain structure. Based on the above-mentioned various theories, the present invention prepares an Al-Zn-Mg alloy with a gradient structure by regulating the Zn alloy and combining the melt stripping method + extrusion composite process, thereby obtaining excellent mechanical properties and damping properties, thereby broadening its industrial application.
[0030] Specifically, the present invention provides a method for preparing a high-strength and high-damping gradient Al-Zn-Mg alloy, comprising the following steps:
[0031] (1) preparing high zinc Al-Zn-Mg strip blanks (Zn content is 20-45wt%, preferably 20wt%, 35wt% or 45wt%), medium zinc Al-Zn-Mg strip blanks (Zn content is 10-18wt%, preferably 10wt%, 14wt% or 18wt%) and low zinc Al-Zn-Mg strip blanks (Zn content is 4-8wt%, preferably 4wt%, 6wt% or 8wt%) by melt spinning method;
[0032] (2) Winding a certain amount of low-zinc Al-Zn-Mg strip blank to form a rod core, then winding a middle-zinc Al-Zn-Mg strip blank on the surface of the rod core, and finally winding a high-zinc Al-Zn-Mg strip blank, and preparing the required rod blank through the above winding; the zinc content of the core, the middle layer and the surface layer is determined according to the needs;
[0033] (3) heating the rod-shaped blank in the above step (2) to 150-250° C. (preferably 200-250° C.), and then compacting it in a hot isostatic press to prepare a strip extruded or rolled rod blank, with a compaction pressure of 200-400 MPa (preferably 200-300 MPa, more preferably 200 MPa) and a holding time of 10-40 min (preferably 10-30 min, more preferably 10 min);
[0034] (4) The rod blank in step (3) is heated to a homogenization temperature (350-420°C, preferably 400°C), kept warm for 0.5-2h, and then densified (hot extrusion is used as an example in the present invention) to prepare the desired gradient Al-Zn-Mg alloy rod. Hot extrusion process parameters: the homogenization temperature and the extrusion temperature are both lower than the melting point of the surface high zinc Al-Zn-Mg alloy, between 350-420°C (preferably 350°C, 400°C or 420°C), the extruder pressure is 400-600t (preferably 450-600t), the extrusion ratio is 10-50 (preferably 12-25), and air cooling is performed after extrusion.
[0035] The raw materials used in the following examples of the present invention are all commercially available.
[0036] The following examples serve as further illustrations of the technical solutions of the present invention.
[0037] Example 1
[0038] (1) Weigh a mixture of industrial pure aluminum, industrial zinc and industrial pure magnesium (wherein the zinc content is 25wt%, the magnesium content is 1.5wt%, and the balance is aluminum content), place the mixture in a crucible, heat it to 700°C to completely melt it, and let it stand for 30 minutes; then spray the alloy melt onto a high-speed rotating copper roller, and rapidly solidify to prepare a fine-grained aluminum alloy strip blank (i.e., a high-zinc Al-Zn-Mg strip blank). The nozzle aperture is 3 mm, the distance from the nozzle to the copper roller is 10 mm, and the strip blank has a thickness of 120 μm and a width of 3 mm.
[0039] Similarly, the above method is used to prepare a medium-zinc Al-Zn-Mg strip blank with a zinc content of 14wt%, a magnesium content of 1.5wt%, and the balance being aluminum content, as well as a low-zinc Al-Zn-Mg strip blank with a zinc content of 6.5wt%, a magnesium content of 1.5wt%, and the balance being aluminum content.
[0040] (2) 200 g of a low zinc Al-Zn-Mg strip blank with a zinc content of 6.5 wt% is used as a core, and 200 g of a medium zinc Al-Zn-Mg strip blank with a zinc content of 14 wt% is wrapped around the core, and finally 200 g of a high zinc Al-Zn-Mg strip blank with a zinc content of 25 wt% is wrapped around the core to make an alloy mixed strip blank, referred to as 25-14-6.5 mixed strip blank;
[0041] (3) heating the billet to 200° C. and then placing it in a hot isostatic pressing device and maintaining the pressure at 200 MPa for 10 min to prepare an extruded billet with a size of Φ55×30 mm;
[0042] (4) The extruded billet was heated to 400°C and kept at this temperature for 1 hour, and then a rod with a diameter of 10 mm was obtained by hot extrusion process. The hot extrusion temperature was 400°C, the die temperature was 380°C, the extruder pressure was 600t, the extrusion ratio was 30, and air cooling was performed after extrusion.
[0043] Example 2
[0044] The same as Example 1, except that the zinc content in the high zinc Al-Zn-Mg strip blank is 45wt%, the zinc content in the medium zinc Al-Zn-Mg strip blank is 18wt%, and the zinc content in the low zinc Al-Zn-Mg strip blank is 4wt%, and a mixed strip blank referred to as 45-18-4 is prepared.
[0045] Example 3
[0046] The same as Example 1, except that the zinc content in the high zinc Al-Zn-Mg strip blank is 20wt%, the zinc content in the medium zinc Al-Zn-Mg strip blank is 10wt%, and the zinc content in the low zinc Al-Zn-Mg strip blank is 8wt%, and a 20-10-8 mixed strip blank is prepared.
[0047] Example 4
[0048] Same as Example 2, except that the hot extrusion temperature is 350°C.
[0049] Example 5
[0050] Same as Example 2, except that the hot extrusion temperature is 420°C.
[0051] Example 6
[0052] Same as Example 3, except that the hot extrusion temperature is 350°C.
[0053] Example 7
[0054] Same as Example 3, except that the hot extrusion temperature is 420°C.
[0055] Comparative Example 1
[0056] The same as Example 1, except that a pure Al-24Zn-1.5Mg alloy strip having a zinc content of 24wt%, a magnesium content of 1.5wt% and the balance being aluminum content is prepared without gradient change, and steps (1) and (2) do not need to be performed, and only steps (3) to (4) are performed using the alloy.
[0057] Comparative Example 2
[0058] The same as Example 1, except that a pure Al-45Zn-1.5Mg alloy strip having a zinc content of 45wt%, a magnesium content of 1.5wt% and the balance being aluminum is prepared without gradient change, and only the alloy is used to perform steps (3)-(4).
[0059] Comparative Example 3
[0060] The same as Example 1, except that an Al-6.5Zn-1.5Mg alloy having a zinc content of 6.5wt%, a magnesium content of 1.5wt% and the balance being aluminum is prepared, and only this alloy is used to carry out steps (3) to (4).
[0061] Comparative Example 4
[0062] Same as Example 1, except that 7075 aluminum alloy is used as raw material to perform operations (3)-(4).
[0063] Comparative Example 5
[0064] Same as Example 1, except that 6061 aluminum alloy is used as raw material to perform operations (3)-(4).
[0065] Comparative Example 6
[0066] Same as Example 1, except that 2014 aluminum alloy is used as raw material to perform operations (3)-(4).
[0067] Comparative Example 7
[0068] The same as Example 1, except that Zn-40Al alloy (i.e., zinc content of 60 wt %, aluminum content of 40 wt %) is used as raw material to carry out operations (3)-(4).
[0069] Comparative Example 8
[0070] The same as Example 1, except that the operations (3) to (4) are performed using Zn-10Al alloy (i.e., a zinc content of 90 wt % and an aluminum content of 10 wt %) as the raw material.
[0071] Comparative Example 9
[0072] The same as Example 1, except that pure Zn is used as the raw material to carry out the operations (3)-(4).
[0073] Comparative Example 10
[0074] Same as Example 1, except that the intermediate layer is not included and the others are the same.
[0075] Comparative Example 11
[0076] Same as Example 1, excluding the surface layer, and the rest are the same.
[0077] Comparative Example 12
[0078] Same as in Example 1, the order of the middle layer and the surface layer is reversed.
[0079] Comparative Example 13
[0080] Same as in Example 1, the order of the core and the surface is reversed.
[0081] Comparative Example 14
[0082] As in Example 1, the order of the core and the middle layer is reversed.
[0083] Figure 1 Schematic diagram of the preparation of high-strength and high-damping gradient Al-Zn-Mg alloy in the present invention. Figure 1 It can be seen that the zinc concentration of the prepared gradient alloy gradually increases from the inside to the outside.
[0084] Figure 2 Schematic diagram of the longitudinal section metallographic structure of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention; Figure 2 It can be seen that the core of the gradient alloy is a typical deformation structure (the grains are elongated along the extrusion direction), the middle is a double-peak grain structure composed of deformation structure and equiaxed crystals, and the surface is a typical recrystallized structure, that is, equiaxed crystals.
[0085] Figure 3 This is the surface equiaxed crystal EBSD grayscale image of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention; Figure 3 It can be seen that the surface presents a typical recrystallized structure, that is, a typical equiaxed crystal structure.
[0086] Figure 4 EBSD grayscale image of the intermediate layer structure of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention; Figure 4 It can be seen that the middle layer is indeed a bimodal grain structure mainly composed of equiaxed grains and deformed grains.
[0087] Figure 5 This is the EBSD grayscale image of the surface equiaxed crystal structure of the high-strength and high-damping gradient Al-Zn-Mg alloy prepared in Example 1 of the present invention. Figure 5 It can be seen that the surface layer is composed of typical equiaxed grains and belongs to the recrystallized grain structure.
[0088] Performance Testing
[0089] (1) Mechanical properties test: The mechanical properties of various alloys were tested using a uniaxial tensile test. The test equipment was an Instron 3369 electronic tensile testing machine with a strain rate of 1×10 -2 / s, and obtain the engineering stress-strain curve. According to the stress-strain curve, the mechanical properties of the material are obtained.
[0090] (2) Damping performance test: A dynamic damping tester was used to test the room temperature damping performance of various alloys. The damping test strain amplitude was 1×10 -4 , the test frequency is 1-10Hz, the test temperature is 25-300℃, and the heating rate is 5℃ / min. Through the temperature and internal friction factor curve, the room temperature damping performance of the material, that is, the internal friction factor, is obtained. Usually, the internal friction factor below 0.01 is defined as a low damping material, and the internal friction factor above 0.01 is defined as a high damping material. The higher the internal friction factor, the better the damping performance.
[0091] Table 1 Mechanical properties and damping properties of alloys prepared in Examples and Comparative Examples
[0092]
[0093] As can be seen from the table, high zinc Al-Zn-(Mg) alloys have excellent damping properties (Comparative Examples 1, 2, 7 and 8), but low strength; low zinc Al-Zn-(Mg) alloys have high strength (Comparative Examples 3, 4, 5 and 6), but poor damping properties; pure zinc has extremely low strength, but excellent damping properties (Comparative Example 9). When there is no intermediate layer or no surface layer, it is difficult for the alloy to obtain ideal strength and damping properties (Comparative Examples 10 and 11); when the core, intermediate layer and surface layer are swapped, it is found that it is difficult to achieve a synergistic improvement in strength and damping (Comparative Examples 12, 13 and 14).
[0094] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A high-strength and high-damping gradient Al-Zn-Mg alloy, characterized in that: The core is made of low-zinc Al-Zn-Mg alloy, the middle layer is made of medium-zinc Al-Zn-Mg alloy, and the surface is made of high-zinc Al-Zn-Mg alloy. The content of Zn in the low-zinc Al-Zn-Mg alloy is 4-8wt%; the content of Zn in the medium-zinc Al-Zn-Mg alloy is 10-18wt%; the content of Zn in the high-zinc Al-Zn-Mg alloy is 20-45wt%; The preparation method of the high-strength and high-damping gradient Al-Zn-Mg alloy comprises the following steps: The low-zinc Al-Zn-Mg alloy strip blank, the medium-zinc Al-Zn-Mg alloy strip blank and the high-zinc Al-Zn-Mg alloy strip blank are prepared by melt spinning method; A rod-shaped blank is prepared by a winding method, wherein the core of the rod-shaped blank is a low-zinc Al-Zn-Mg alloy strip blank, the middle layer is a medium-zinc Al-Zn-Mg alloy strip blank, and the surface is a high-zinc Al-Zn-Mg alloy strip blank; The rod-shaped billet is made into an extruded billet by a hot isotropic extrusion method; then the extruded billet is homogenized and hot extruded to obtain a high-strength and high-damping gradient Al-Zn-Mg alloy.
2. The high-strength and high-damping gradient Al-Zn-Mg alloy according to claim 1, characterized in that: The parameters of the hot isostatic extrusion method are: temperature 150-250° C., pressure 200-400 MPa, and holding time 10-40 min.
3. The high-strength and high-damping gradient Al-Zn-Mg alloy according to claim 1, characterized in that: The homogenization refers to keeping the temperature at 350-420° C. for 0.5-2 h.
4. The high-strength and high-damping gradient Al-Zn-Mg alloy according to claim 1, characterized in that: The parameters of the hot extrusion are: temperature 350-420°C, pressure 400-600t, and extrusion ratio 10-50.
5. Use of the high-strength and high-damping gradient Al-Zn-Mg alloy according to any one of claims 1 to 4 in the preparation of national defense, military industry, and aerospace components.