A fire-resistant and flame-retardant cable

By combining modified low-melting-point ceramic powder with a PVC matrix, numerous continuous carbonized mesh insulation layers are formed, solving the problem of brittle fracture of fire-resistant cables in fire environments, achieving both cable toughness and safety, and reducing manufacturing and installation difficulties.

CN118280648BActive Publication Date: 2024-11-15TIANHUAN CABLE GRP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410611616.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-11-15
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Existing fire-resistant cables become brittle with low-melting-point glass powder in fire environments, causing the cable surface to crumble and posing a risk of leakage. Furthermore, the manufacturing process is complex, costly, and inconvenient to install.

Method used

Modified low-melting-point ceramic powder is used as a flame retardant material. It is modified by replacing chloropropyltriethoxysilane with diethyl iminodiacetate, transesterifying diethylenetriamineamine, and grafting DOPO to form a fire-resistant protective layer. Combined with the PVC matrix, it forms numerous continuous carbonized network isolation layers to avoid glass phase brittleness.

Benefits of technology

It achieves a protective layer that is tough and does not easily break in a fire environment, maintains cable safety, reduces cable weight and manufacturing complexity, and improves ease of installation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to a fire-resistant flame-retardant cable, belonging to the technical field of special flame-retardant cables. The cable at least comprises a wire core and a fire-resistant protective layer on its surface, wherein the fire-resistant protective layer comprises by weight: 100 parts of PVC resin, 12-16 parts of POE resin, 35-42 parts of modified low-melting-point porcelain powder, 18-24 parts of plasticizer, 3.2-3.8 parts of stabilizer, 3.5-5 parts of lubricant and 3-4 parts of masterbatch; in a fire ablation environment, DOPO on the surface of the modified low-melting-point porcelain powder is preferentially decomposed to form a carbonization-promoting phosphide, which in situ promotes carbonization of its near-surface layer to form a carbonized network with high temperature stability, avoiding the formation of a continuous brittle glass phase layer, but using countless continuous glass phase-carbonized network insulation layers to hinder the deepening of combustion, and compared with a continuous glass phase insulation layer, it has higher toughness, and for non-fixed cables, it is not easy to collapse during the movement process after ablation, resulting in protection failure and leakage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of special flame-retardant cables, and in particular relates to a fire-resistant flame-retardant cable. Background Art

[0002] Cables are carriers for transmitting electrical signals and electric currents, and the stability of their power supply will directly determine the operational safety of the equipment. With the improvement of people's awareness of fire safety, the continuous increase in high-rise buildings, large supermarkets, hospitals, stations, and airports, the construction of subways, tunnels, and public transportation, and the increase in large-scale public sports and entertainment facilities, the importance of fire protection and fire safety has become more prominent. In a fire scene, ensuring the safety of electricity and the smooth flow of communications is an important factor in reducing casualties and loss of life and property. As a special cable, fire-resistant cables have good fire resistance. Traditional fire-resistant cables are isolated and fire-proofed by setting a magnesium oxide mineral layer or mica tape between the protective surface and the core. This type of cable has good fire resistance, but the manufacturing process is complicated, the cost is high, and the cable is heavy, making it inconvenient to lay and install. In the prior art, various flame retardants are compounded with polymer materials to make flame retardant materials as fireproof layers, which can meet certain flame retardant requirements. Among them, polymer materials doped with low-melting point glass powder have better fire resistance. Under the high temperature environment of fire, the polarity of low-melting point glass powder undergoes glass transition and aggregation to form a fire-resistant glass phase insulation layer with good fire-resistant insulation. However, the formed glass phase is very brittle. For some non-fixed cables, such as elevator cables and hoist cables, the cables move with the work during operation. The surface layer becomes brittle after fire erosion and collapses during the movement and deformation process. Failure of protection can easily lead to secondary damage caused by leakage. Summary of the invention

[0003] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a fire-resistant and flame-retardant cable.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A fire-resistant flame-retardant cable comprises at least a core and a fire-resistant protective layer on the surface thereof, wherein the fire-resistant protective layer comprises, by weight:

[0006] 100 parts of PVC resin, 12-16 parts of POE resin, 35-42 parts of modified low melting point porcelain powder, 18-24 parts of plasticizer, 3.2-3.8 parts of stabilizer, 3.5-5 parts of lubricant and 3-4 parts of masterbatch.

[0007] The modified low melting point porcelain powder is prepared by the following method:

[0008] Step A1: diethyl iminodiacetate, triethoxysilane chloropropyl, triethylamine and anhydrous acetone were mixed, nitrogen was introduced for protection, the temperature was raised to 50-60° C., mechanical stirring was applied at 120-180 rpm, and refluxed for 3.5-4 h. After the reaction was completed, acetone was evaporated to obtain intermediate 1;

[0009] Furthermore, the usage ratio of diethyl iminodiacetate, chloropropyltriethoxysilane, triethylamine and anhydrous acetone is 0.1 mol: 0.1 mol: 5-7 mL: 60-80 mL. Under the promotion of triethylamine, chloropropyltriethoxysilane is substituted with diethyl iminodiacetate to form a silane containing a diethyl acetate structure.

[0010] Step A2: Mix the intermediate 1, diethylenetriamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 45-55°C, apply mechanical stirring at 60-90 rpm, add sodium hydride intermittently, and control the total reaction time to be 6-8 hours. After the reaction is completed, distill off the tetrahydrofuran to obtain the intermediate 2;

[0011] Furthermore, the usage ratio of intermediate 1, diethylenetriamine, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.2 mol: 0.15-0.21 g: 120-160 mL. Under the promotion of strong base sodium hydride, diethylenetriamine and the diethyl diacetate structure of intermediate 1 undergo amine ester exchange to introduce active amino group modification.

[0012] Step A3: Mix the intermediate 2 and the ethanol solution, adjust the pH value to 4.5-5.5 with formic acid, add low melting point glass powder, heat to 40-50°C, ultrasonically shake for 30-40 minutes, neutralize with ammonia water after cooling, let stand for 24 hours, take the bottom precipitate, wash with water and dry to obtain the amino base powder;

[0013] Furthermore, the amount ratio of the low-melting-point glass powder, the intermediate 2 and the ethanol solution is 100 g: 4.2-5.5 g: 130-180 mL, the ethanol solution is an ethanol aqueous solution with a mass fraction of 60%, and the ethoxysilane structure in the molecular structure of the intermediate 2 is hydrolyzed and coupled with the surface of the low-melting-point glass powder, so that the intermediate 2 molecule is grafted onto the surface;

[0014] Furthermore, the initial melting temperature of the low-melting-point glass powder is 400-500°C.

[0015] Step A4: DOPO, triethylamine and dichloromethane are mixed, and the amino base powder is added for ultrasonic dispersion. The temperature is controlled at 10-20°C in an ice-water bath, and stirring is applied at 60-90 rpm. Carbon tetrachloride is slowly added, and the total reaction time is controlled to be 10-12 hours. After the reaction is completed, the precipitate is allowed to stand, washed with water and dried to obtain a modified low-melting-point porcelain powder;

[0016] Furthermore, the dosage ratio of the amino base powder, DOPO, carbon tetrachloride, triethylamine and dichloromethane is 100g:6.5-8.2g:4-6mL:10-15mL:220-260mL. Under the promotion of carbon tetrachloride, DOPO reacts with the active amino groups in the amino base powder to graft DOPO to the surface.

[0017] A fire-resistant and flame-retardant cable is made by the following method:

[0018] Step S1: taking the raw materials according to the weight ratio and mixing them evenly, kneading them at 160±10° C. until the torque is stable, and extruding and pelletizing them to obtain a composite masterbatch;

[0019] Step S2: Extruding and coating the composite masterbatch on the surface of the wire core, cooling and forming, winding, baking to relieve stress, forming a fire-resistant protective layer on the surface of the wire core, and obtaining a fire-resistant flame-retardant cable.

[0020] Furthermore, during the extrusion coating process, the barrel temperature of the twin-screw extruder is set to: 170-180°C in zone 1, 185-195°C in zone 2, 190-200°C in zone 3, 165-175°C in zone 4, and the head temperature is 180-195°C.

[0021] Beneficial effects of the present invention:

[0022] The invention discloses a PVC-based protective fire-resistant cable, wherein the flame retardant grade of the fire-resistant protective layer reaches V-0, and the ablated layer after ablation has good toughness and is not easy to break and cause leakage; a modified low-melting-point porcelain powder is introduced into the fire-resistant protective layer as a flame retardant material, wherein the low-melting-point glass powder is used as a carrier, chloropropyltriethoxysilane and diethyl iminodiacetate are substituted, and then diethylenetriamine and ester are subjected to amine ester exchange, and loaded onto the surface of the low-melting-point glass powder through coupling action, and finally DOPO is reacted with the introduced amino group to graft DOPO onto the surface; the organic multiamide structure of the surface layer of the modified low-melting-point porcelain powder modifies the low-melting-point glass powder, and has good wettability with the PVC matrix. Smooth dispersibility, easy to evenly disperse into the matrix during the melt blending process; in the fire ablation environment, its surface DOPO preferentially decomposes to form carbonization-promoting phosphides, which in situ promotes the carbonization of its near-surface layer to form a carbonized network with high temperature stability. Different from the traditional low-melting-point glass flame retardant form, the carbonized network separates the low-melting-point glass particles to prevent them from agglomerating to form a continuous brittle glass phase layer. It is an innumerable continuous glass phase-carbonized network insulation layer that hinders the deepening of combustion. Compared with the continuous glass phase insulation layer, it has higher toughness, so that the ablated layer after ablation has a certain toughness. For non-fixed cables, it is not easy to break during the movement after ablation, resulting in protection failure and leakage. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1, preparing a fire-resistant flame-retardant cable, specifically as follows:

[0025] 1) Preparation of modified low melting point ceramic powder

[0026] Step A1: Mix diethyl iminodiacetate, triethyl chloropropylsilane, triethylamine and anhydrous acetone, introduce nitrogen protection, heat to 60°C, apply mechanical stirring at 180 rpm, and reflux for 3.5 hours, wherein the amount ratio of diethyl iminodiacetate, triethyl chloropropylsilane, triethylamine and anhydrous acetone is 0.1 mol: 0.1 mol: 5 mL: 80 mL. After the reaction is completed, acetone is evaporated to obtain intermediate 1.

[0027] Step A2: Mix the intermediate 1, diethylenetriamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 55°C, apply mechanical stirring at 90rpm, take equal mass of sodium hydride and divide it into three parts, add it intermittently for 1h, and control the total addition reaction time of sodium hydride to be 6h, wherein the amount ratio of intermediate 1, diethylenetriamine, sodium hydride and anhydrous tetrahydrofuran is 0.1, mol: 0.2mol: 0.15g: 160mL. After the reaction, distill off tetrahydrofuran to obtain intermediate 2.

[0028] Step A3: prepare a 60% mass fraction of ethanol aqueous solution, mix the intermediate 2 and the ethanol solution, adjust the pH value to 4.5 with formic acid, add low melting point glass powder, and use D240 raw material from Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd. during the implementation process. The initial melting temperature is 400°C, the temperature is raised to 50°C, ultrasonically oscillated at 28kHz for 30min, and neutralized with ammonia water after cooling, and allowed to stand for 24h. The amount ratio of low melting point glass powder, intermediate 2 and ethanol solution is 100g:5.5g:180mL. Take the bottom precipitate, wash with water and dry to obtain amino base powder.

[0029] Step A4: DOPO, triethylamine and dichloromethane are mixed, and the amino base powder is added and ultrasonically dispersed at 28kHz. The temperature is controlled to 20°C in an ice-water bath, and stirring is applied at 90rpm. Carbon tetrachloride is slowly added within 3 hours, and the total reaction time of carbon tetrachloride addition is controlled to be 10 hours. The amount ratio of the amino base powder, DOPO, carbon tetrachloride, triethylamine and dichloromethane is 100g:8.2g:6mL:15mL:260mL. After the reaction is completed, the precipitate is allowed to stand, washed with water and dried to obtain a modified low-melting-point porcelain powder.

[0030] 2) Cable preparation

[0031] Step S1: Take the raw materials according to weight parts, 100 parts of PVC resin, SG-3 resin of Shanxi Yushe Chemical Co., Ltd. is used in the implementation process; 12 parts of POE resin, 65057 resin of Wanhua Chemical is used in the implementation process; 35 parts of modified low melting point porcelain powder, prepared by this embodiment; 24 parts of plasticizer, industrial grade DOP is used in the implementation process; 3.8 parts of stabilizer, TCS-108A-B calcium zinc stabilizer of Shandong Jinchang Resin New Material Technology Co., Ltd. is used in the implementation process; 3.5 parts of lubricant, G60 raw material of Jiangsu Qingfu New Material Technology Co., Ltd. is used in the implementation process; 3 parts of masterbatch, H7 raw material of Dongguan Ruijia Plastic Technology Co., Ltd. is used in the implementation process; mix the raw materials, put them into an internal mixer, mix them at 160±10°C until the torque is stable, extrude and pelletize to obtain a composite masterbatch.

[0032] Step S2: The composite masterbatch is transferred into an extruder, and plasticized and extruded by a twin-screw extruder to be coated on the surface of the wire core, wherein the barrel temperature of the twin-screw extruder is set to: 180°C for zone 1, 195°C for zone 2, 200°C for zone 3, 175°C for zone 4, and the head temperature is 195°C. After cooling and molding, the wire is rolled up, and baked at 60°C for 2 hours to remove stress, forming a fire-resistant protective layer on the surface of the wire core to obtain a fire-resistant flame-retardant cable.

[0033] Example 2, preparing a fire-resistant flame-retardant cable, as follows:

[0034] 1) Preparation of modified low melting point ceramic powder

[0035] Step A1: Mix diethyl iminodiacetate, triethyl chloropropylsilane, triethylamine and anhydrous acetone, introduce nitrogen protection, heat to 50°C, apply mechanical stirring at 120 rpm, and reflux for 4 hours, wherein the amount ratio of diethyl iminodiacetate, triethyl chloropropylsilane, triethylamine and anhydrous acetone is 0.1 mol: 0.1 mol: 7 mL: 60 mL. After the reaction is completed, acetone is evaporated to obtain intermediate 1.

[0036] Step A2: Mix the intermediate 1, diethylenetriamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 45°C, apply mechanical stirring at 60rpm, take equal mass of sodium hydride and divide it into three parts, add it intermittently for 1h, and control the total addition reaction time of sodium hydride to be 8h, wherein the amount ratio of intermediate 1, diethylenetriamine, sodium hydride and anhydrous tetrahydrofuran is 0.1, mol: 0.2mol: 0.21g: 120mL. After the reaction, distill off tetrahydrofuran to obtain intermediate 2.

[0037] Step A3: prepare a 60% mass fraction ethanol aqueous solution, mix the intermediate 2 and the ethanol solution, adjust the pH value to 5.5 with formic acid, add low melting point glass powder, and use FD66A raw material from Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd. during the implementation process. The initial melting temperature is 500°C, the temperature is raised to 40°C, ultrasonically oscillated at 28kHz for 40min, and after cooling, it is neutralized with ammonia water and allowed to stand for 24h. The amount ratio of low melting point glass powder, intermediate 2 and ethanol solution is 100g:4.2g:130mL. Take the bottom precipitate, wash with water and dry to obtain the amino base powder.

[0038] Step A4: DOPO, triethylamine and dichloromethane are mixed, and the amino base powder is added and ultrasonically dispersed at 28kHz. The temperature is controlled at 10°C in an ice-water bath, and stirring is applied at 60rpm. Carbon tetrachloride is slowly added within 4 hours, and the total reaction time of carbon tetrachloride is controlled to be 10-12 hours. The amount ratio of the amino base powder, DOPO, carbon tetrachloride, triethylamine and dichloromethane is 100g:6.5g:4mL:10mL:220mL. After the reaction is completed, the precipitate is allowed to stand, washed with water and dried to obtain a modified low-melting-point porcelain powder.

[0039] 2) Cable preparation

[0040] Step S1: Take raw materials according to weight parts, 100 parts of PVC resin, SG-3 resin of Shanxi Yushe Chemical Co., Ltd. is used in the implementation process; 16 parts of POE resin, 65057 resin of Wanhua Chemical is used in the implementation process; 42 parts of modified low melting point porcelain powder, prepared by this embodiment; 18 parts of plasticizer, industrial grade DOP is used in the implementation process; 3.2 parts of stabilizer, TCS-108A-B calcium zinc stabilizer of Shandong Jinchang Resin New Material Technology Co., Ltd. is used in the implementation process; 4.5 parts of lubricant, G60 raw material of Jiangsu Qingfu New Material Technology Co., Ltd. is used in the implementation process; 4 parts of masterbatch, H7 raw material of Dongguan Ruijia Plastic Technology Co., Ltd. is used in the implementation process; mix the raw materials, put them into an internal mixer, mix them at 160±10°C until the torque is stable, extrude and pelletize to obtain a composite masterbatch.

[0041] Step S2: The composite masterbatch is transferred into an extruder, and plasticized and extruded by a twin-screw extruder to be coated on the surface of the wire core, wherein the barrel temperature of the twin-screw extruder is set to: 170°C for zone 1, 185°C for zone 2, 190°C for zone 3, 165°C for zone 4, and the head temperature is 180°C. After cooling and molding, the masterbatch is rolled up, and baked at 60°C for 2 hours to remove stress, forming a fire-resistant protective layer on the surface of the wire core to obtain a fire-resistant flame-retardant cable.

[0042] Example 3, preparing a fire-resistant flame-retardant cable, as follows:

[0043] 1) Preparation of modified low melting point ceramic powder

[0044] Step A1: Mix diethyl iminodiacetate, chloropropyltriethoxysilane, triethylamine and anhydrous acetone, introduce nitrogen protection, heat to 58°C, apply mechanical stirring at 180 rpm, and reflux for 3.7 hours, wherein the amount ratio of diethyl iminodiacetate, chloropropyltriethoxysilane, triethylamine and anhydrous acetone is 0.1 mol: 0.1 mol: 6 mL: 75 mL. After the reaction is completed, acetone is evaporated to obtain intermediate 1.

[0045] Step A2: Mix the intermediate 1, diethylenetriamine and anhydrous tetrahydrofuran, introduce nitrogen protection, heat to 52°C, apply mechanical stirring at 90rpm, take equal mass of sodium hydride and divide it into three parts, add it intermittently for 1h, and control the total addition reaction time of sodium hydride to be 7h, wherein the amount ratio of intermediate 1, diethylenetriamine, sodium hydride and anhydrous tetrahydrofuran is 0.1, mol: 0.2mol: 0.18g: 150mL. After the reaction, distill off tetrahydrofuran to obtain intermediate 2.

[0046] Step A3: prepare a 60% mass fraction ethanol aqueous solution, mix the intermediate 2 and the ethanol solution, adjust the pH value to 5 with formic acid, add low melting point glass powder, and use D245 raw material from Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd. during the implementation process. The initial melting temperature is 450°C, the temperature is raised to 45°C, ultrasonically oscillated at 28kHz for 35min, and neutralized with ammonia water after cooling, and allowed to stand for 24h. The amount ratio of low melting point glass powder, intermediate 2 and ethanol solution is 100g:5g:150mL. Take the bottom precipitate, wash with water and dry to obtain amino base powder.

[0047] Step A4: DOPO, triethylamine and dichloromethane are mixed, and the amino base powder is added and ultrasonically dispersed at 28kHz. The temperature is controlled to be 15°C in an ice-water bath, and stirring is applied at 90rpm. Carbon tetrachloride is slowly added within 3.5 hours, and the total reaction time of carbon tetrachloride addition is controlled to be 11 hours. The amount ratio of the amino base powder, DOPO, carbon tetrachloride, triethylamine and dichloromethane is 100g:7.5g:5mL:12mL:250mL. After the reaction is completed, the precipitate is allowed to stand, washed with water and dried to obtain a modified low-melting-point porcelain powder.

[0048] 2) Cable preparation

[0049] Step S1: Take raw materials according to weight parts, 100 parts of PVC resin, SG-3 resin of Shanxi Yushe Chemical Co., Ltd. is used in the implementation process; 14 parts of POE resin, 65057 resin of Wanhua Chemical is used in the implementation process; 38 parts of modified low melting point porcelain powder, prepared by this embodiment; 20 parts of plasticizer, industrial grade DOP is used in the implementation process; 3.5 parts of stabilizer, TCS-108A-B calcium zinc stabilizer of Shandong Jinchang Resin New Material Technology Co., Ltd. is used in the implementation process; 5 parts of lubricant, G60 raw material of Jiangsu Qingfu New Material Technology Co., Ltd. is used in the implementation process; 3 parts of masterbatch, H7 raw material of Dongguan Ruijia Plastic Technology Co., Ltd. is used in the implementation process; mix the raw materials, load them into an internal mixer, mix them at 160±10°C until the torque is stable, extrude and pelletize to obtain a composite masterbatch.

[0050] Step S2: The composite masterbatch is transferred into an extruder, and plasticized and extruded by a twin-screw extruder to be coated on the surface of the wire core, wherein the barrel temperature of the twin-screw extruder is set to: 175°C for zone 1, 190°C for zone 2, 195°C for zone 3, 170°C for zone 4, and the head temperature is 190°C. After cooling and forming, the wire is rolled up and baked at 60°C for 2 hours to remove stress, forming a fire-resistant protective layer on the surface of the wire core to obtain a fire-resistant flame-retardant cable.

[0051] In a comparative example, low melting point glass powder and DOPO composite modified PVC were used to prepare fire-resistant flame-retardant cables. The specific implementation process is as follows:

[0052] The raw materials are taken by weight: 100 parts of PVC resin, SG-3 resin of Shanxi Yushe Chemical Co., Ltd. is used in the implementation process; 14 parts of POE resin, 65057 resin of Wanhua Chemical is used in the implementation process; 38 parts of low-melting point glass powder, D245 raw material of Anmi Micro-Nano New Materials (Guangzhou) Co., Ltd.; 1.5 parts of DOPO, industrial-grade raw material; 24 parts of plasticizer, industrial-grade DOP is used in the implementation process; 3.5 parts of stabilizer, TCS-108A-B calcium zinc stabilizer of Shandong Jinchang Resin New Materials Technology Co., Ltd. is used in the implementation process; 5 parts of lubricant, G60 raw material of Jiangsu Qingfu New Materials Technology Co., Ltd. is used in the implementation process; 3 parts of masterbatch, H7 raw material of Dongguan Ruijia Plastic Technology Co., Ltd. is used in the implementation process; the specific process for preparing the cable is the same as Example 3.

[0053] In order to detect the protective effect of the fire-resistant protective layer of the fire-resistant flame-retardant cable, the molten material extruded in the above extrusion process was transferred into the mold, solidified by unidirectional pressing at 2.5MPa, demolded after cooling, and made into a film. After stress relief, the tensile performance test was carried out in accordance with GB / T 1040.1-2018, and the film was reciprocatedly ablated for 10 minutes with an alcohol burner, and stretched again to measure the tensile strength and elongation at break retention rate; the flame retardant performance test was carried out using a UL94 burning test machine; the specific test results are shown in Table 1:

[0054] Table 1

[0055]

[0056] It can be seen from the test results in Table 1 that the protective layers of the cables prepared in the embodiments and the comparative examples meet the V-0 flame retardant requirements and have good flame retardancy. After the ablation test, the tensile strength retention rate of the embodiments is 44.2-50.9 MPa, and the elongation at break retention rate is 51.4-59.1%. The tensile strength retention rate of the comparative example is 71.4%, and the elongation at break retention rate is 13.5%. It can be seen that after ablation, the protective layer of the comparative example shows obvious brittleness. After fire ablation, the protective layer is too brittle and easy to peel off, which can easily cause leakage accidents.

[0057] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0058] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A fire-resistant flame-retardant cable, comprising at least a core and a fire-resistant protective layer on its surface, characterized in that: The fire-resistant protective layer includes, by weight: 100 parts of PVC resin, 12-16 parts of POE resin, 35-42 parts of modified low-melting-point porcelain powder, 18-24 parts of plasticizer, 3.2-3.8 parts of stabilizer, 3.5-5 parts of lubricant and 3-4 parts of masterbatch; The modified low melting point porcelain powder is prepared by the following method: Step A1: diethyl iminodiacetate, triethoxysilane chloropropyl, triethylamine and anhydrous acetone are mixed, nitrogen is introduced for protection, the temperature is raised to 50-60°C, and the mixture is stirred and refluxed for reaction for 3.5-4h. After the reaction is completed, the acetone is evaporated to obtain intermediate 1; Step A2: Mix the intermediate 1, diethylenetriamine and anhydrous tetrahydrofuran, introduce nitrogen protection, raise the temperature to 45-55°C, stir and add sodium hydride intermittently, control the total reaction time to be 6-8h, and evaporate the tetrahydrofuran after the reaction to obtain the intermediate 2; Step A3: Mix the intermediate 2 and the ethanol solution, adjust the pH value to 4.5-5.5 with formic acid, add low melting point glass powder, heat to 40-50°C, ultrasonically shake for 30-40 minutes, neutralize with ammonia water after cooling, let stand for 24 hours, take the bottom precipitate, wash with water and dry to obtain the amino base powder; Step A4: DOPO, triethylamine and dichloromethane are mixed, and the amino base powder is added for ultrasonic dispersion. The temperature is controlled at 10-20°C in an ice-water bath. Carbon tetrachloride is slowly added while stirring. The total reaction time is controlled to be 10-12h. After the reaction is completed, the precipitate is allowed to stand, washed with water and dried to obtain a modified low-melting-point porcelain powder.

2. A fire-resistant and flame-retardant cable according to claim 1, characterized in that: In step A1, the usage ratio of diethyl iminodiacetate, chloropropyltriethoxysilane, triethylamine and anhydrous acetone is 0.1 mol: 0.1 mol: 5-7 mL: 60-80 mL.

3. A fire-resistant and flame-retardant cable according to claim 2, characterized in that: The usage ratio of intermediate 1, diethylenetriamine, sodium hydride and anhydrous tetrahydrofuran is 0.1, mol: 0.2 mol: 0.15-0.21 g: 120-160 mL.

4. A fire-resistant and flame-retardant cable according to claim 3, characterized in that: The dosage ratio of the low-melting-point glass powder, the intermediate 2 and the ethanol solution is 100 g: 4.2-5.5 g: 130-180 mL, and the ethanol solution is an ethanol aqueous solution with a mass fraction of 60%.

5. A fire-resistant and flame-retardant cable according to claim 4, characterized in that: The initial melting temperature of low melting point glass powder is 400-500℃.

6. A fire-resistant and flame-retardant cable according to claim 4, characterized in that: In step A4, the usage ratio of the amination base powder, DOPO, carbon tetrachloride, triethylamine and dichloromethane is 100 g: 6.5-8.2 g: 4-6 mL: 10-15 mL: 220-260 mL.

7. A fire-resistant and flame-retardant cable according to claim 1, characterized in that: Made by: Step S1: taking the raw materials according to the weight ratio and mixing them evenly, kneading them at 160±10° C. until the torque is stable, and extruding and pelletizing them to obtain a composite masterbatch; Step S2: Extruding and coating the composite masterbatch on the surface of the wire core, cooling and forming, winding, baking to relieve stress, forming a fire-resistant protective layer on the surface of the wire core, and obtaining a fire-resistant flame-retardant cable.

8. A fire-resistant and flame-retardant cable according to claim 7, characterized in that: During the extrusion coating process, the barrel temperature of the twin-screw extruder was set to: 170-180°C in zone 1, 185-195°C in zone 2, 190-200°C in zone 3, 165-175°C in zone 4, and the die head temperature was 180-195°C.

Citation Information

Patent Citations

  • Composite particles having hydrophobicity and heat-resistant flame-retardant performance as well as preparation method thereof

    CN104961849A

  • Low-smoke halogen-free flame-retardant cable

    CN116386943A

  • Fireproof flame-retardant cable and preparation method thereof

    CN116462922A

  • Mineral cable and preparation method thereof

    CN117936177A