A long-lasting functionalized double-layer bionic small-caliber artificial blood vessel and its preparation method and application
Through a three-step solution polymerization method and thermally induced phase separation technology based on the principle of 'bulk copolymerization', a double-layer bionic small-diameter artificial blood vessel that can sustainably release DSS, NO and H2S was prepared, solving the problem of insufficient release of functional factors in the existing technology. problem, achieving rapid remodeling and functional repair of vascular tissue.
Patent Information
- Application Number
- CN202410451145.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-04-16
AI Technical Summary
Existing small-diameter artificial blood vessels are difficult to achieve long-term release of functional factors due to functional bionic modification, resulting in functional loss after early rapid release. Moreover, the surface grafting sites are limited, making it difficult to load more functional factors, resulting in insufficient remodeling of vascular tissue.
A three-step solution polymerization method based on the principle of 'bulk copolymerization' is used to synthesize degradable polyurethane materials. The inner layer of axially oriented fibrous blood vessels is spun by near-field direct writing and the outer layer of axially oriented topological microstructured blood vessels is prepared by thermally induced phase separation technology. Realize the continuous release of DSS, NO and H2S throughout the life cycle, and dynamically regulate the microenvironment of vascular tissue.
The preparation of long-lasting functional double-layer bionic small-diameter artificial blood vessels has been achieved. The active molecules in the inner and outer layers interact to strengthen the interaction, quickly promote the remodeling of vascular tissue, inhibit inflammation and oxidative stress, protect endothelial cells, and achieve long-distance vascular tissue regeneration and function. Reshaping.
Smart Images

Figure CN118304471B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of using biomaterials for vascular tissue engineering, and particularly relates to a long-acting functionalized double-layer bionic small-caliber artificial blood vessel and a preparation method and application thereof. Background Art
[0002] Cardiovascular disease (CVD) has always been the leading cause of death worldwide. The 2023 World Heart Report released by the World Heart Federation (WHF) shows that in 2021, the number of deaths caused by cardiovascular disease accounted for about one-third of the total number of deaths worldwide. In China, the prevalence of CVD is also in a stage of continuous increase, ranking first in the proportion of disease deaths among urban and rural residents. Clinically, small-caliber vascular injuries and lesions are very common. Replacing the diseased blood vessels through vascular transplantation surgery is an important means of treating cardiovascular and orthopedic vascular injury diseases. However, small-caliber artificial blood vessels (inner diameter ≤6mm) have slow blood flow, easy thrombosis, and low long-term patency. There are still no mature products on the market in China or even globally. It is very important and urgent to develop small-caliber artificial blood vessels with long-term anticoagulation, inhibition of proliferation and long-term patency.
[0003] In the process of vascular tissue regeneration, regulating the physiological microenvironment of damaged or diseased blood vessels is a crucial link in promoting vascular tissue regeneration and functional remodeling. Danshensu (DSS) can dynamically regulate oxidative stress, and selenium compounds can catalyze the endogenous donor nitrosothiol (RSNO) to continuously release NO, thereby inhibiting platelet adhesion / activation and promoting the repair of damaged endothelial tissue. At the same time, NO can promote the endogenous synthesis of H2S by smooth muscle cells, and H2S can further promote the decomposition of RSNO to release NO. At present, there is no report on the biodegradable polyurethane small-caliber artificial blood vessels synthesized based on "bulk copolymerization" with good comprehensive mechanical properties and the ability to dynamically regulate the "full life cycle" release of DSS, NO or H2S in situ.
[0004] Small-caliber artificial blood vessels modified with degradable polyurethane have excellent mechanical compliance and mechanical strength, and have significant advantages in terms of process, cost, production conditions, and storage conditions. They can be used to induce vascular tissue regeneration in situ in vivo. However, it is difficult to achieve controlled release of functional factors in existing artificial blood vessels with bionic functional modifications. Early rapid release often leads to functional loss in the later stage, or it is difficult to load more functional factors due to limited surface grafting sites. In addition, as the surface material degrades in the early stage, the unfunctionalized part is exposed, resulting in early endothelial degeneration, making it difficult to achieve long-distance vascular tissue remodeling. Therefore, small-caliber artificial blood vessel materials are in urgent need of long-term functional modification to solve the problem of pathological remodeling caused by insufficient functionalization.
[0005] In summary, the preparation of a long-lasting functional double-layer bionic small-caliber artificial blood vessel that can dynamically respond to the repair microenvironment is of great significance in the field of medical devices and biomedicine. Its application and promotion can fill the current market gap of small-caliber artificial blood vessels, alleviate the tension of clinical small-caliber blood vessel transplantation, and bring huge economic and social benefits. Summary of the invention
[0006] In order to solve the above problems, the main purpose of the present invention is to provide a method for preparing a long-lasting functional double-layer bionic small-caliber artificial blood vessel, including synthesizing a mechanically matched degradable polyurethane artificial blood vessel material capable of long-term release of active components through a three-step solution polymerization method based on the "bulk copolymerization principle", spinning an axially oriented fiber vascular inner layer through near-field direct writing, and preparing an axially oriented topological microstructured vascular outer layer through a special mold combined with thermally induced phase separation technology.
[0007] Another object of the present invention is to provide a long-acting functionalized double-layer bionic small-caliber artificial blood vessel, which is prepared by the preparation method of the long-acting functionalized double-layer bionic small-caliber artificial blood vessel, and has the function of continuously releasing DSS, NO and H2S with interactive reinforcing effects during the "whole life cycle", as well as in situ dynamic regulation and repair of the vascular tissue microenvironment.
[0008] Another object of the present invention is to provide the application of the long-acting functionalized double-layer bionic small-caliber artificial blood vessel as or in the preparation of a medical product that can dynamically regulate and repair the microenvironment.
[0009] To achieve the above object, the present invention adopts the following technical solution:
[0010] The present invention provides a method for preparing a long-acting functionalized double-layer bionic small-caliber artificial blood vessel, comprising the following steps:
[0011] (1) Based on bulk copolymerization, biodegradable polyurethane elastomers PCHU-DSeSe and PCHU-DTA were synthesized by a three-step solution polymerization method. The synthetic monomers included soft segment diols and diisocyanates, as well as chain extenders, to keep the weight average molecular weight of PCHU-DSeSe and PCHU-DTA elastomers between 80,000 and 100,000 and the viscosity coefficient between 1.2 and 1.8;
[0012] (2) electrospinning the PCHU-DSeSe in step (1) on a stainless steel shaft core having axial grooves of a mold by near-field direct writing to obtain PCHU-DSeSe oriented fibers as the axially oriented fiber vascular inner layer, wherein the fiber diameter is controlled between 0.1 and 80 μm, and the fiber and the shaft core are placed in a vacuum drying oven and dried for at least 2 days;
[0013] (3) assembling the axially oriented fiber vascular inner layer with the shaft core compounded in step (2) into a polytetrafluoroethylene mold having radially oriented patterns on the inner wall of the shell;
[0014] (4) Weighing PCHU-DTA, dissolving it in dimethyl sulfoxide (DMSO) at 50-60° C., stirring and dissolving to obtain a clear and uniform solution of 8-16% (mass volume ratio, w / v), and quickly casting the solution into the polytetrafluoroethylene mold with the oriented fiber layer in step (3), and quickly placing it at -80° C. to allow thermally induced phase separation to occur for more than 48 hours, thereby obtaining an outer layer of a blood vessel with an axially oriented topological microstructure;
[0015] (5) taking out the mold, removing the outer shell of the mold and immersing it in a 0°C ultrapure ice-water mixture for 10 minutes to obtain an artificial blood vessel, and then removing it from the axis of the mold and continuing to immerse it in a 0°C ultrapure ice-water mixture. The water is changed every 4 hours to exchange the solvent, and the water is changed 6 to 10 times in total; the artificial blood vessel is taken out from the deionized water and freeze-dried for more than 3 days to obtain a long-lasting functional double-layer bionic small-caliber artificial blood vessel.
[0016] Preferably, in step (1), the molar ratio of the synthetic monomers of the degradable polyurethane elastomers PCHU-DSeSe and PCHU-DTA, namely, the soft segment diol, the diisocyanate and the chain extender is 1:2:1.
[0017] Preferably, in step (1), the soft segment diol is selected from one or more of polycaprolactone diol (HO-PCL-OH), polycarbonate diol (HO-PC-OH), polylactic acid diol (HO-PLLA-OH), poly(lactic acid-glycolic acid) diol (HO-PLGA-OH), poly(lactic acid-caprolactone) diol (HO-PLCL-OH), and poly(glycolic acid-caprolactone) diol (HO-PGCL-OH).
[0018] Preferably, in step (1), the diisocyanate is selected from one or more of toluene diisocyanate (TDI), isophorone diisocyanate (IPDI), diphenylmethane diisocyanate (MDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and lysine diisocyanate (LDI).
[0019] Preferably, in step (1), the chain extender used in the synthesis monomers of the degradable polyurethane elastomers PCHU-DSeSe and PCHU-DTA includes chain extender 1 and chain extender 2; wherein the chain extender 1 used in the synthesis of PCHU-DSeSe is danshensu (DSS), and the chain extender 2 used is selected from one or more of 2-(2-hydroxyethyl diselenol)ethanol (SeDO), selenocystamine hydrochloride (SeCA), 3,3'-di(diselenide)dipropionic acid (SeDPA), 4,4'-dithiodiylbis(4,1-phenylene)dimethanol, bis(4-carboxyphenyl) diselenide, and bis(4-aminophenyl) diselenide); the chain extender 1 used in the synthesis of PCHU-DTA is danshensu (DSS), and the chain extender 2 used is O-hydroxymethyl-2-hydroxythioacetate (TA); the order of adding the chain extenders is: first add chain extender 1 and then add chain extender 2.
[0020] More preferably, in step (1), the molar ratio of chain extender 1 to chain extender 2 used in the synthetic monomers of PCHU-DSeSe is 1:99 to 99:1.
[0021] More preferably, in step (1), the chain extender used in the PCHU-DTA is DSS and TA in a molar ratio of 1:99 to 99:1.
[0022] Preferably, in step (1), during the synthesis reaction of PCHU-DSeSe and PCHU-DTA, the reaction temperature of the soft segment diol and the diisocyanate is 50-80° C., the stirring rate is 80-250 rpm, and the reaction time is 2-3 h.
[0023] Preferably, in step (1), during the synthesis reaction of PCHU-DSeSe and PCHU-DTA, DSS is dissolved in DMSO and added dropwise, and the concentration of DSS / DMSO solution is controlled at 0.02-0.01 g / mL, with the optimal concentration being 0.04 g / mL; the dripping speed is 8-12 mL / h, with the optimal speed being 10 mL / h.
[0024] Preferably, in step (1), during the synthesis reaction of PCHU-DSeSe and PCHU-DTA, the stirring rate after adding the chain extender is controlled at 500-800 rpm, the reaction time after adding DSS is controlled at 3-5 h, the chain extender 2 is dissolved in DMAc and triethylamine (TEA) is added dropwise as an acid binding agent, and then the chain extender 2 / DMAc / TEA is added dropwise to the prepolymer, 0.1 mL of TEA is added dropwise to each milliliter of the chain extender 2 / DMAc solution, and the concentration of the chain extender 2 / DMAc solution is 0.02-0.01 g / mL, the dropping rate is 8-12 mL / h, and the reaction time in each reaction is 8-24 h.
[0025] Preferably, in step (2), when preparing the axially oriented fiber vascular inner layer by near-field direct writing electrospinning, the shaft core speed is 10-18 rpm and the needle moving speed is 800-1200 mm / min.
[0026] Preferably, the inner and outer layer sizes of the long-acting functional double-layer bionic small-caliber artificial blood vessel are controllably adjusted through electrospinning and molds, and are controlled to: the inner diameter (d1) is 1.2-6 mm, the total wall thickness (T) is 0.1-3 mm, the inner layer PCHU-DSeSe oriented fiber thickness (t1) is 0.05-1.5 mm, the outer layer oriented topological microstructure PCHU-DTA porous material thickness (t2) is 0.05-2 mm, and the artificial blood vessel length (L) is controlled to be 0.5-25 cm; the outer layer thread profile is triangular or trapezoidal, the ratio of the thread height (h) to the total wall thickness (T) of the artificial blood vessel is 1:5-10, the number of threads is 1-2, the pitch is 0.1-2 mm, and the lead is 0.1-4 mm.
[0027] The present invention also provides a long-acting functionalized double-layer bionic small-caliber artificial blood vessel, which is prepared by the preparation method of the long-acting functionalized double-layer bionic small-caliber artificial blood vessel.
[0028] The present invention also provides the use of the long-acting functionalized double-layer bionic small-caliber artificial blood vessel as or in the preparation of a medical product for arteriovenous fistula, coronary artery and peripheral vascular bypass treatment.
[0029] Preferably, the long-acting functionalized double-layer bionic small-caliber artificial blood vessel has the function of continuously releasing DSS, NO and H2S during the "entire life cycle" and dynamically regulating and repairing the microenvironment of vascular tissue in situ.
[0030] Compared with the prior art, the beneficial effects of the present invention are at least:
[0031] 1. Based on the principle of bulk copolymerization, the present invention prepares two degradable polyurethane elastomers PCHU-DSeSe and PCHU-DTA by a three-step solution polymerization method. They have good biocompatibility, processability and mechanical elasticity, low preparation cost, simple process and controllable performance.
[0032] 2. The long-acting functionalized double-layer bionic small-caliber artificial blood vessel of the present invention has the inner layer continuously releasing DSS and NO, and the outer layer continuously releasing DSS and H2S, and the active molecules released from the inner and outer layers can interact and enhance the effect, realize the synergistic effect of the two, and dynamically regulate and repair the microenvironment of vascular tissue in situ, which can quickly promote vascular tissue remodeling.
[0033] 3. In the present invention, the long-lasting functional double-layer bionic small-caliber artificial blood vessel obtains an axially oriented inner surface of the fiber through electrospinning, which effectively realizes the recruitment of endothelial cells and promotes the migration and proliferation of endothelial cells; the oriented porous structure outer surface obtained by thermally induced phase separation not only improves the anti-bending effect of blood vessels, but also can dynamically regulate the migration and proliferation of smooth muscle cells; the inner and outer layers of the artificial blood vessel can continuously release DSS, respond to the inflammatory and oxidative stress microenvironment, effectively inhibit related adverse reactions, and protect endothelial cells and smooth muscle cells from damage.
[0034] 4. The long-acting functionalized double-layer bionic small-caliber artificial blood vessels of the present invention can be used for arteriovenous fistula, coronary artery and peripheral vascular bypass treatment. The PCHU-DSeSe oriented fibers in the inner layer of the blood vessels can in situ catalyze the endogenous NO source to continuously release NO, and the outer layer oriented topological microstructure PCHU-DTA degradable polyurethane porous material can controllably degrade and release H2S, NO and H2S, which can interactively promote and regulate vascular function.
[0035] 5. The long-acting functionalized double-layer bionic small-caliber artificial blood vessels of the present invention have adjustable mechanical compliance, bursting strength and biocompatibility, have no hypersensitivity reaction to the human body during transplantation surgery, and have affinity with the blood and surrounding tissues in the human body. After transplantation, the release of active small molecules can be regulated during the entire degradation cycle, the endothelial cell layer can be quickly and stably reshaped to achieve long-term anticoagulation, the microenvironment can be dynamically regulated to repair, and the regeneration and functional remodeling of long-distance small-caliber vascular tissue can be quickly achieved. It has a good application prospect in cardiovascular surgery, hemodialysis center, nephrology, and orthopedic repair surgery. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Schematic diagram of the synthesis reaction of the degradable polyurethane elastomer PCHU-DSeSe for preparing oriented fibers for the inner layer of artificial blood vessels by the "three-step solution polymerization method" in Example 1.
[0037] Figure 2 Schematic diagram of the synthesis reaction of the degradable polyurethane elastomer PCHU-DTA for preparing the oriented topological microstructure porous material of the outer layer of artificial blood vessels by the "three-step solution polymerization method" in Example 1.
[0038] Figure 3 Schematic diagram of the preparation process of the long-lasting functional double-layer bionic small-caliber artificial blood vessel in the embodiment.
[0039] Figure 4 Schematic diagram of the biological regulation mechanism of the long-acting functional double-layer bionic small-caliber artificial blood vessel in the embodiment.
[0040] Figure 5 The long-acting functionalized double-layer bionic small-caliber artificial blood vessel prepared in the embodiment and its X-ray diffraction electron microscope image, wherein Figure 5A is a photo of the prepared long-lasting functional double-layer bionic small-caliber artificial blood vessel. Figure 5 B is the cross-sectional view, Figure 5 C is a longitudinal section, 5D is a cross-sectional view of the lumen, Figure 5 E is the scanned image of the outer surface. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0042] Example 1
[0043] In this embodiment, a long-acting functional double-layer bionic small-caliber artificial blood vessel is prepared. The soft segment diol of the synthetic monomer of the degradable polyurethane elastomer PCHU-DSeSe is HO-PCL-OH, the diisocyanate is HDI, the chain extender 2 is SeDO, and the molar ratio of the chain extender 1 to the chain extender 2 is 1:3; the soft segment diol of the synthetic monomer of the degradable polyurethane elastomer PCHU-DTA is HO-PCL-OH, the diisocyanate is HDI, and the molar ratio of DSS to TA is 1:3. The steps are as follows:
[0044] (1) The specific operation of preparing the degradable polyurethane elastomers PCHU-DSeSe and PCHU-DTA by three-step solution polymerization based on the principle of bulk copolymerization is as follows: weigh 5g of polycaprolactone diol (PCL diol, Mn is 2000) in a 250mL three-necked flask, stir at 180rpm for 10min at 60℃; then heat to 120℃ to remove water in vacuum for 30min, then pass nitrogen protection and cool to 60℃; take 0.81mL HDI and add it to the three-necked flask to react for 2.5h; then cool to 45℃, adjust the speed to 560rpm, weigh 0.12g DSS and dissolve it completely with 5mL DMSO and drip it into the three-necked flask drop by drop, and drip it in about 30min, continue to stir and react for 3h, and add about 10mL DMSO during the reaction according to the change of solution viscosity; weigh 0.47g SeDO and dissolve it with 10mL DMSO and drip it into the three-necked flask drop by drop and continue to react for 12h according to the change of viscosity during the reaction. DMSO; after stopping the reaction, the polymer was precipitated with deionized water and the solvent was exchanged for 48 hours, and the deionized water was replaced every 6 hours, and the deionized water was replaced 8 times in total to completely wash away the DMSO; the washed material was then taken out and frozen at -80°C for 3 hours, and then freeze-dried to obtain PCHU-DSeSe. The preparation process of PCHU-DTA is the same as that of PCHU-DSeSe, except that 0.47g of SeDO is changed to 0.23g of TA, the reaction solvent is DMAc, and the reaction pH needs to be adjusted by adding TEA, and finally PCHU-DTA is prepared.
[0045] (2) Weigh 0.35 g of PEO and dissolve it in 10 mL of deionized water until it is completely dissolved to obtain a release layer spinning solution. A uniform PEO release layer is obtained on a shaft core with a diameter of 3 mm by near-field direct writing, and the solution is left overnight to evaporate the water. Weigh 0.8 g of PCHU-DSeSe and dissolve it in 10 mL of hexafluoroisopropanol (HFIP). After it is completely dissolved, the PCHU-DSeSe / HFIP solution is electrospun at a shaft core speed of 10 rpm and a needle moving speed of 1000 mm / min to obtain an axially oriented artificial blood vessel inner layer with a thickness of 0.4 mm after vacuum drying.
[0046] (3) The axially oriented fiber tube with the axial core composited in step (2) is assembled into a mold shell with an inner diameter of 5 mm and a polytetrafluoroethylene mold with radially oriented lines (triangular thread, number of threads is 1, pitch is 1 mm, thread height is 0.2 mm) on the inner wall for standby use; then 0.8 g of PCHU-DTA is weighed on an analytical balance, dissolved in 10 mL of DMSO at 60° C., stirred to dissolve, and a clear and uniform solution is obtained. Subsequently, the mixed solution is quickly cast into a polytetrafluoroethylene mold of a specific model with an oriented fiber layer assembled, and quickly placed at -80° C. for phase separation, and the placement time is more than 48 hours. Then take out the mold, remove the outer shell of the mold and immerse it in a 0℃ ultrapure ice water mixture. After 10 minutes, remove the artificial blood vessel from the core of the mold and continue to immerse it in a 0℃ ultrapure ice water mixture. Change the water and solvent every 4 hours, and change the water 6 to 10 times in total. After taking out the artificial blood vessel from the deionized water, freeze-dry it for more than 3 days to obtain a double-layer bionic small-caliber artificial blood vessel with an inner diameter of about 3 mm and a thickness of about 1 mm.
[0047] Example 2
[0048] In this embodiment, a long-acting functional double-layer bionic small-caliber artificial blood vessel is prepared. The soft segment of the synthetic monomer of the degradable polyurethane elastomer PCHU-DSeSe is HO-PC-OH, the diisocyanate is HDI, the chain extender 2 is SeDO, and the molar ratio of the chain extender 1 to the chain extender 2 is 1:1; the soft segment of the synthetic monomer of PCHU-DTA is HO-PCL-OH, the diisocyanate is HDI, and the molar ratio of DSS to TA is 1:1. The operation steps are as follows:
[0049] (1) The specific operation of preparing PCHU-DSeSe and PCHU-DTA by three-step solution polymerization based on the principle of bulk copolymerization is as follows: weigh 5g of polycarbonate diol (PC diol, Mn ~ 2000) in a 250mL three-necked flask, stir at 180rpm for 10min at 60℃; then heat to 120℃ and remove water in vacuum for 30min, then pass nitrogen protection and cool to 60℃; take 0.81mL HDI and add it to the three-necked flask to react for 2.5h; then cool to 45℃, adjust the speed to 560rpm, weigh 0.24g DSS and dissolve it completely with 10mL DMSO and drip it into the three-necked flask drop by drop, and drip it in about 50min, continue to stir and react for 3h, and add about 10mL DMSO during the reaction according to the change of solution viscosity; then weigh 0.11g SeDO and dissolve it with 6mL DMSO and drip it into the three-necked flask drop by drop and continue to react for 12h according to the change of viscosity during the reaction. DMSO; after stopping the reaction, the polymer was precipitated with deionized water and the solvent was exchanged for 48 hours, and the deionized water was replaced every 6 hours, and the deionized water was replaced 8 times in total to completely wash away the DMSO; the washed material was then taken out and frozen at -80°C for 3 hours, and then freeze-dried to obtain PCHU-DSeSe. The preparation process of PCHU-DTA is the same as that of PCHU-DSeSe, except that 0.47g of SeDO is changed to 0.15g of TA, the reaction solvent is DMAc, and the reaction pH needs to be adjusted by adding TEA, and finally PCHU-DTA is prepared.
[0050] (2) Weigh 0.35 g of PEO and dissolve it in 10 mL of deionized water until it is completely dissolved to obtain a release layer spinning solution. A uniform PEO release layer is obtained on a shaft core with a diameter of 3 mm by near-field direct writing, and the solution is left overnight to evaporate the water. Weigh 1 g of PCHU-DSeSe and dissolve it in 10 mL of hexafluoroisopropanol (HFIP). After it is completely dissolved, the PCHU-DSeSe / HFIP solution is electrospun at a shaft core speed of 12 rpm and a needle moving speed of 1200 mm / min to obtain an axially oriented artificial vascular inner layer with a thickness of 0.4 mm after vacuum drying.
[0051] (3) The axially oriented fiber tube with the axial core composited in step (2) is assembled into a mold shell with an inner diameter of 5 mm and a polytetrafluoroethylene mold with radially oriented lines (triangular thread, number of threads is 1, pitch is 1 mm, thread height is 0.2 mm) on the inner wall for standby use; then 1 g of PCHU-DTA is weighed on an analytical balance, dissolved in 10 mL of DMSO at 60° C., and stirred to dissolve to obtain a clear and uniform solution. Subsequently, the mixed solution is quickly cast into a previously assembled polytetrafluoroethylene mold of a specific model with an oriented fiber layer, and quickly placed at -80° C. for phase separation, and the placement time is more than 48 hours. Then take out the mold, remove the outer shell of the mold and immerse it in a 0°C ultrapure ice water mixture. After 10 minutes, remove the artificial blood vessel from the axis of the mold and continue to immerse it in a 0°C ultrapure ice water mixture. Change the water and solvent every 4 hours, and change the water 6 to 10 times in total. After taking out the artificial blood vessel from the deionized water, freeze-dry it for more than 3 days to obtain a double-layer bionic small-caliber artificial blood vessel with an inner diameter of about 3 mm and a thickness of about 1 mm.
[0052] Comparative Example 1
[0053] The difference between this comparative example and Example 1 is that the molar ratio of chain extender 1 to chain extender 2 during the synthesis of PCHU-DSeSe is 15:85; the molar ratio of DSS to TA during the synthesis of PCHU-DTA is 15:85.
[0054] Comparative Example 2
[0055] The difference between this comparative example and Example 1 is that the molar ratio of chain extender 1 to chain extender 2 during the synthesis of PCHU-DSeSe is 35:65; the molar ratio of DSS to TA during the synthesis of PCHU-DTA is 35:65.
[0056] Comparative Example 3
[0057] The difference between this comparative example and Example 1 is that the molar ratio of chain extender 1 to chain extender 2 during the synthesis of PCHU-DSeSe is 1:1; and the molar ratio of DSS to TA during the synthesis of PCHU-DTA is 1:1.
[0058] Comparative Example 4
[0059] The difference between this comparative example and Example 1 is that the molar ratio of chain extender 1 to chain extender 2 during the synthesis of PCHU-DSeSe is 65:35; and the molar ratio of DSS to TA during the synthesis of PCHU-DTA is 65:35.
[0060] Comparative Example 5
[0061] The difference between this comparative example and Example 1 is that the molar ratio of chain extender 1 to chain extender 2 during the synthesis of PCHU-DSeSe is 75:25; the molar ratio of DSS to TA during the synthesis of PCHU-DTA is 75:25.
[0062] Comparative Example 6
[0063] The difference between this comparative example and Example 1 is that the molar ratio of chain extender 1 to chain extender 2 during the synthesis of PCHU-DSeSe is 85:15; the molar ratio of DSS to TA during the synthesis of PCHU-DTA is 85:15.
[0064] Performance Testing
[0065] The long-acting functionalized double-layer bionic small-caliber artificial blood vessels prepared in the above-mentioned examples and comparative examples were subjected to radial mechanical tensile testing and endothelial coverage statistics, and the inner layer fiber orientation was observed by scanning electron microscopy (SEM).
[0066] Radial mechanical tensile test
[0067] All samples of the embodiments and comparative examples were cut into the same length (5 mm) for radial mechanical tensile test. Before the tensile test, all samples were immersed in 0.01 M phosphate buffer (PBS, pH = 6.8) at 37 ° C for 24 h. A tensile tester (HY-940FS) was used, and radial uniaxial tension test was performed, with a sensor load range of 0-200 N and a tensile speed of 1 mm / min.
[0068] Endothelial coverage test
[0069] Test method: The PCHU-DSeSe of the embodiment and the comparative example was prepared into an oriented fiber membrane of 24 wells and sterilized and then laid on the bottom of a 24-well plate. In each well of the 24-well plate, a specially made sterile 316L stainless steel bar was stacked vertically on the fiber membrane in the orientation direction to divide the well into two parts. Then, HUVECs primary cells were evenly inoculated into the 24-well plate (1×10 5 / well). After 12 hours of culture, the steel bar was removed and cultured for another 48 hours. After 48 hours, the cells were fixed with 4% paraformaldehyde for more than 2 hours and washed with PBS 3 to 5 times; rhodamine-labeled phalloidin was added and incubated at room temperature in the dark for 1.5 hours, and washed with PBS 3 to 5 times; DAPI staining solution was used for 5 minutes in the dark, and washed with PBS 3 to 5 times. Finally, the cell migration morphology and the migration distance of the stained cell nucleus compared with the original state were observed under an inverted fluorescence microscope, and the cell coverage percentage was calculated by Image J software, endothelial coverage percentage (%) = cell coverage area / original area of the well plate × 100%.
[0070] Table 1: Performance test results of examples and comparative examples
[0071]
[0072]
[0073] As shown in Table 1, only by controlling the ratio of DSS and chain extender 2 to TA and the processing parameters, can a long-lasting functionalized double-layer bionic small-caliber artificial blood vessel with matching mechanical properties and effective synergistic effects of NO and H2S be prepared through three-step solution polymerization, electrospinning and thermally induced phase separation technology. It can stably and long-term dynamically regulate the vascular transplantation microenvironment in situ, achieve rapid endothelialization effect, shorten the vascular remodeling cycle, and realize long-distance vascular tissue regeneration.
[0074] The above is a preferred embodiment of the present invention, but the present invention should not be limited to the contents disclosed in the embodiment. Therefore, any equivalent or modification completed without departing from the spirit disclosed in the present invention shall fall within the scope of protection of the present invention.
Claims
1. A method for preparing a long-lasting functionalized double-layer bionic small-caliber artificial blood vessel, characterized in that: The following steps are involved: (1) Based on bulk copolymerization, biodegradable polyurethane elastomers PCHU-DSeSe and PCHU-DTA were synthesized by a three-step solution polymerization method. The synthetic monomers included soft segment diol and diisocyanate, and also included a chain extender. The molar ratio of the soft segment diol, diisocyanate and chain extender was 1:2:
1. Keep the weight average molecular weight of PCHU-DSeSe and PCHU-DTA between 80,000 and 100,000, and the viscosity coefficient between 1.2 and 1.8; (2) PCHU-DSeSe in step (1) is electrospinned by near-field direct writing on a stainless steel shaft core with axial grooves of a mold to obtain PCHU-DSeSe oriented fibers as the axially oriented fiber vascular inner layer, with a fiber diameter between 0.1 and 80 μm, and the fibers and the shaft core are vacuum dried as a whole for at least 2 days; (3) assembling the axially oriented fiber vascular inner layer with the shaft core compounded in step (2) into a polytetrafluoroethylene mold having radially oriented patterns on the inner wall of the outer shell; (4) Weigh PCHU-DTA, dissolve it in DMSO at 50-60°C, stir and dissolve to obtain a clear and uniform solution of 8-16 w / v%, quickly cast the solution into the polytetrafluoroethylene mold assembled in step (3), and quickly place it at -80°C to allow thermally induced phase separation to occur for at least 48 hours to obtain an outer layer of a vascular topological microstructure oriented around the axis; (5) taking out the mold, removing the mold shell and immersing it in a 0°C ultrapure ice water mixture for 10 minutes to obtain a prefabricated artificial blood vessel; removing it from the axis of the mold and continuing to immerse it in a 0°C ultrapure ice water mixture, changing the water and solvent every 4 hours, and changing the water 6 to 10 times in total; taking out the artificial blood vessel from the 0°C ultrapure ice water and freeze-drying it for no less than 3 days to obtain a long-lasting functional double-layer bionic small-caliber artificial blood vessel; In step (1), the soft segment diol is selected from HO-PCL-OH; The diisocyanate is selected from HDI; The chain extenders used in the synthesis of PCHU-DSeSe and PCHU-DTA include chain extender 1 and chain extender 2; The chain extender 1 used in the synthesis of PCHU-DSeSe is DSS, and the chain extender 2 is selected from 2-(2-hydroxyethyl diselenide)ethanol; The chain extender 1 used in the synthesis of PCHU-DTA is DSS, and the chain extender 2 is TA; The order of adding the chain extender is: first add chain extender 1 and then add chain extender 2, and the molar ratio of chain extender 1 to chain extender 2 is 1:3; The inner and outer layer sizes of the long-acting functional double-layer bionic small-caliber artificial blood vessel are controllably adjusted through electrospinning and molds, and are controlled to be: the inner diameter is 1.2~6mm, the total wall thickness is 0.1~3mm, the thickness of the inner layer PCHU-DSeSe oriented fiber is 0.05~1.5mm; the thickness of the outer layer oriented topological microstructure PCHU-DTA porous material is 0.05~2mm, and the length of the artificial blood vessel is 0.5~25cm; the outer layer thread tooth shape is triangular or trapezoidal, the ratio of the thread tooth height to the total wall thickness of the artificial blood vessel is 1:5~10, the number of threads is 1~2, the pitch is 0.1~2mm, and the lead is 0.1~4mm; The long-acting functionalized double-layer bionic small-caliber artificial blood vessel has the function of continuously releasing DSS and NO throughout the "whole life cycle", and the outer layer continuously releases DSS and H2S. The active molecules released from the inner and outer layers can interactively enhance the effects, as well as the function of dynamically regulating and repairing the microenvironment of vascular tissue in situ.
2. The method for preparing the long-acting functionalized double-layer bionic small-caliber artificial blood vessel according to claim 1, characterized in that: In step (2), when preparing the axially oriented fiber vascular inner layer by near-field direct writing electrospinning, the shaft core speed is 10-18 rpm and the needle moving speed is 800-1200 mm / min.
Citation Information
Patent Citations
Selenium-containing polyurethane with stable and controllable release of nitric oxide, preparation method and application thereof
CN109651586A
Double-layer artificial blood vessel and preparation method thereof
CN110124108A