A heterojunction battery adhesive film and preparation method thereof

By using a specific raw material formulation and ultraviolet irradiation crosslinking technology, a heterojunction battery encapsulant film with an interpenetrating network structure is formed, which solves the problems of poor adhesion and insufficient resistance to damp heat aging in existing technologies. This achieves good adhesion and efficient encapsulation with HJT solar cells, thereby improving the photoelectric conversion efficiency and service life of the battery.

CN118308037BActive Publication Date: 2024-11-19HAOCHEN WUXI PLASTIC IND CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410510076.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-26
Publication Date
2024-11-19
Estimated Expiration
2044-04-26

AI Technical Summary

Technical Problem

Existing heterojunction battery encapsulants have poor adhesion to HJT cells, insufficient resistance to damp heat aging, high film fluidity, and poor encapsulation effect, resulting in poor encapsulation effect and mechanical properties, which affect the photoelectric conversion efficiency and service life of the battery.

Method used

A specific raw material formulation is used, including EVA resin, 2,4-diphenyl-4-methyl-1-pentene, 2,4,6-trivinylcycloboroxane, 3-(1,1-difluoro-2-propen-1-yl)-2(1H)-quinoxalone, etc., which are cross-linked by ultraviolet light irradiation to form an interpenetrating network structure, thereby improving the adhesion and resistance to damp heat aging of the film.

Benefits of technology

The prepared heterojunction battery encapsulant film has good adhesion to HJT battery cells, strong resistance to damp heat aging, low film flowability, and excellent mechanical properties, which significantly improves the encapsulation effect and extends the battery's service life and photoelectric conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005008605850000061
    Figure GDA0005008605850000061
Patent Text Reader

Abstract

The invention discloses a heterojunction battery adhesive film and a preparation method thereof, which is prepared from the following raw materials: 100 parts of EVA resin, 2-4 parts of 2,4-diphenyl-4-methyl-1-pentene, 1-3 parts of 2,4,6-trivinyl cycloboroxane, 0.8-1.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 3-5 parts of N-vinyl oxazolidinone, 1,3- 3-5 parts of bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 0.5-1 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1-2 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 0.3-0.8 parts of photoinitiator, 0.5-0.8 parts of defoamer, and 0.1-0.4 parts of antioxidant. The adhesive film has good adhesion, resistance to wet and hot aging, and good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of heterojunction batteries, and in particular to a heterojunction battery adhesive film and a preparation method thereof. Background Art

[0002] Against the backdrop of carbon neutrality, carbon peak, and the prominent energy crisis, countries around the world are increasingly aware of the importance of clean energy. As a common hybrid solar cell, heterojunction cells (HJT) have attracted widespread attention due to their many advantages such as cleanliness and environmental protection, simple structure, low process temperature, good passivation effect, high open circuit voltage and photoelectric conversion efficiency, and excellent temperature characteristics. They occupy an extremely important position in the domestic market.

[0003] Heterojunction battery film is one of the most important materials in the promotion and use of heterojunction battery components. Its main function is to protect solar cells and tightly bond the cells to glass, backplane and other materials into a whole. The performance of heterojunction battery film directly affects the photoelectric conversion efficiency and cycle life of heterojunction batteries. However, the existing packaging films have more or less technical defects such as poor adhesion to HJT battery cells, insufficient resistance to moisture and heat aging, high film fluidity leading to wire slippage, and the packaging effect and yellowing resistance need to be further improved.

[0004] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN112980340B discloses a packaging film for encapsulating HJT cells, a preparation method thereof, and a photovoltaic module obtained. The packaging film for encapsulating HJT cells includes an adhesive layer and an EVA layer; the adhesive layer is mainly made of the following components in parts by weight: 100 parts of base resin, 5 to 10 parts of modified resin, and 1 to 5 parts of auxiliary agent; the modified resin is mainly made by reacting base resin, initiator and bonding monomer. The invention introduces a specific modified resin into the adhesive layer to adapt the viscosity-increasing mechanism of the packaging film to the composite ITO anti-reflection light-trapping layer on the surface of HJT, so as to achieve complete bonding between the film and the heterojunction cell, and improve the peeling strength between the film and the HJT cell; at the same time, the EVA layer has a strong peeling strength to the tempered glass or backplane surface, which improves the long-term reliability and service life of the HJT module. However, its resistance to wet and hot aging still needs to be further improved.

[0005] It can be seen that the development of a heterojunction battery film and its preparation method with good adhesion to HJT battery cells, sufficient resistance to moisture and heat aging, low film fluidity, significant packaging effect, and good mechanical properties meets market demand, has broad market value and application prospects, and is of great significance to promoting the development of the HJT battery field. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a heterojunction battery adhesive film and a preparation method thereof which has good adhesion to HJT battery cells, sufficient resistance to moisture and heat aging, low film fluidity, significant packaging effect, and excellent mechanical properties.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a heterojunction battery adhesive film is made of the following raw materials in parts by weight: 100 parts of EVA resin, 2-4 parts of 2,4-diphenyl-4-methyl-1-pentene, 1-3 parts of 2,4,6-trivinyl cycloboroxane, 0.8-1.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, and 0.5-1.5 parts of N-vinyl oxazolidinone. 3-5 parts, 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione 3-5 parts, 1,4-diamino-2,3-dicyanoanthraquinone 0.5-1 parts, 3,3'-diamino-4,4'-difluorodiphenyl sulfone 1-2 parts, photoinitiator 0.3-0.8 parts, defoamer 0.5-0.8 parts, antioxidant 0.1-0.4 parts.

[0008] Preferably, the antioxidant is at least one of antioxidant 1010 and antioxidant 168.

[0009] Preferably, the defoamer is at least one of defoamer AT-99 and defoamer D6800.

[0010] Preferably, the photoinitiator is at least one of benzoin ethyl ether, benzoin isopropyl ether, diphenyl acetone, and 2,4-dihydroxybenzophenone.

[0011] Preferably, the EVA resin is EVA provided by Taiwan Polymer Chemicals Co., Ltd. UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28%, and the melt flow rate is 25g / 10min.

[0012] Another object of the present invention is to provide a method for preparing the heterojunction battery film, comprising the following steps: mixing the raw materials uniformly by weight, extruding through a single-screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet irradiation cross-linking to obtain the heterojunction battery film.

[0013] Preferably, the thickness of the heterojunction battery film is 0.5-1.2 mm.

[0014] Preferably, the ultraviolet light wavelength of the ultraviolet light irradiation is 220-260nm, and the irradiation time is 5-10min.

[0015] Due to the application of the above technical solution, the present invention has the following beneficial effects:

[0016] (1) The method for preparing the heterojunction battery film disclosed in the present invention has simple process, convenient operation and control, high preparation efficiency and finished product qualification rate, low dependence on equipment, low energy consumption, suitable for continuous large-scale production, and has high promotion and application value.

[0017] (2) The heterojunction battery adhesive film disclosed in the present invention is made of the following raw materials in parts by weight: 100 parts of EVA resin, 2-4 parts of 2,4-diphenyl-4-methyl-1-pentene, 1-3 parts of 2,4,6-trivinyl cycloboroxane, 0.8-1.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 3-5 parts of N-vinyl oxazolidinone, 1, 3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione 3-5 parts, 1,4-diamino-2,3-dicyanoanthraquinone 0.5-1 parts, 3,3'-diamino-4,4'-difluorodiphenyl sulfone 1-2 parts, photoinitiator 0.3-0.8 parts, defoamer 0.5-0.8 parts, antioxidant 0.1-0.4 parts. Through the mutual cooperation between the raw materials, the prepared adhesive film has good adhesion to the HJT battery cell, good resistance to moisture and heat aging, low fluidity of the adhesive film, significant encapsulation effect, and good mechanical properties.

[0018] (3) The heterojunction battery adhesive film disclosed in the present invention can undergo a photocuring reaction under the initiation of a photoinitiator by irradiating with ultraviolet light, and the monomer containing unsaturated olefinic bonds and the EVA resin can undergo an epoxy ring-opening reaction with the raw material containing an epoxy group, thereby forming an interpenetrating network structure, giving the adhesive film more excellent resistance to wet heat aging and mechanical properties, effectively improving the packaging effect, and reducing the fluidity of the adhesive film. Through the above reaction, EVA, cycloboroxane, fluoroquinoxaline, oxazolidinone, triazone, cyanoanthraquinone and fluorodiphenyl sulfone structures are simultaneously introduced into the molecular structure of the adhesive film. These structures can further improve the resistance to wet heat aging, adhesion and mechanical properties under the effects of electronic effects, steric effects and conjugation effects, thereby improving the packaging effect and effectively extending the service life of the adhesive film, thereby making the heterojunction battery using the adhesive film more excellent in photoelectric conversion efficiency and cycle life. DETAILED DESCRIPTION

[0019] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0020] Example 1

[0021] A heterojunction battery adhesive film is made of the following raw materials in parts by weight: 100 parts of EVA resin, 2 parts of 2,4-diphenyl-4-methyl-1-pentene, 1 part of 2,4,6-trivinyl cycloboroxine, 0.8 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 3 parts of N-vinyl oxazolidinone, 3 parts of 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 0.5 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1 part of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 0.3 parts of photoinitiator, 0.5 parts of defoamer and 0.1 parts of antioxidant.

[0022] The antioxidant is antioxidant 1010; the defoamer is defoamer AT-99; the photoinitiator is benzoin ethyl ether; the EVA resin is EVA provided by China Taiwan Polymer Chemical Co., Ltd. UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28%, and the melt flow rate is 25g / 10min.

[0023] A method for preparing the heterojunction battery film comprises the following steps: uniformly mixing the raw materials by weight, extruding the raw materials through a single-screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet irradiation cross-linking to obtain the heterojunction battery film; the thickness of the heterojunction battery film is 0.8 mm; the ultraviolet wavelength of the ultraviolet irradiation is 220 nm, and the irradiation time is 5 min.

[0024] Example 2

[0025] A heterojunction battery adhesive film is made of the following raw materials in parts by weight: 100 parts of EVA resin, 2.5 parts of 2,4-diphenyl-4-methyl-1-pentene, 1.5 parts of 2,4,6-trivinyl cycloboroxine, 1 part of 3-(1,1-difluoro-2-propene-1-yl)-2(1H)-quinoxalinone, 3.5 parts of N-vinyl oxazolidinone, 3.5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 0.6 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1.2 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 0.5 parts of photoinitiator, 0.6 parts of defoamer and 0.2 parts of antioxidant.

[0026] The antioxidant is antioxidant 168; the defoamer is defoamer D6800; the photoinitiator is benzoin isopropyl ether; the EVA resin is EVA provided by Taiwan Polymer Chemical Co., Ltd. UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28%, and the melt flow rate is 25g / 10min.

[0027] A method for preparing the heterojunction battery film comprises the following steps: uniformly mixing the raw materials by weight, extruding the raw materials through a single-screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet irradiation cross-linking to obtain the heterojunction battery film; the thickness of the heterojunction battery film is 0.8 mm; the ultraviolet wavelength of the ultraviolet irradiation is 230 nm, and the irradiation time is 7 min.

[0028] Example 3

[0029] A heterojunction battery adhesive film is made of the following raw materials in parts by weight: 100 parts of EVA resin, 3 parts of 2,4-diphenyl-4-methyl-1-pentene, 2 parts of 2,4,6-trivinyl cycloboroxine, 1.2 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 4 parts of N-vinyl oxazolidinone, 4 parts of 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 0.8 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1.5 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 0.5 parts of photoinitiator, 0.65 parts of defoamer and 0.25 parts of antioxidant.

[0030] The antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 3:5; the defoamer is a mixture of defoamer AT-99 and defoamer D6800 in a mass ratio of 1:2; the photoinitiator is diphenyl acetophenone; the EVA resin is EVA provided by Taiwan Polymer Chemical Co., Ltd. UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28%, and the melt flow rate is 25g / 10min.

[0031] A method for preparing the heterojunction battery film comprises the following steps: uniformly mixing the raw materials by weight, extruding the raw materials through a single-screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet irradiation cross-linking to obtain the heterojunction battery film; the thickness of the heterojunction battery film is 0.8 mm; the ultraviolet wavelength of the ultraviolet irradiation is 240 nm, and the irradiation time is 8 min.

[0032] Example 4

[0033] A heterojunction battery adhesive film is made of the following raw materials in parts by weight: 100 parts of EVA resin, 3.5 parts of 2,4-diphenyl-4-methyl-1-pentene, 2.5 parts of 2,4,6-trivinyl cycloboroxine, 1.3 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 4.5 parts of N-vinyl oxazolidinone, 4.5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 0.9 parts of 1,4-diamino-2,3-dicyanoanthraquinone, 1.8 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 0.7 parts of photoinitiator, 0.75 parts of defoamer and 0.35 parts of antioxidant.

[0034] The antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:3; the defoamer is a mixture of defoamer AT-99 and defoamer D6800 in a mass ratio of 1:3; the photoinitiator is a mixture of benzoin ethyl ether, benzoin isopropyl ether, diphenyl acetone, and 2,4-dihydroxybenzophenone in a mass ratio of 1:2:2:1; the EVA resin is EVA provided by Taiwan Polymer Chemical Co., Ltd. UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28%, and the melt flow rate is 25g / 10min.

[0035] A method for preparing the heterojunction battery film comprises the following steps: uniformly mixing the raw materials by weight, extruding the raw materials through a single-screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet irradiation cross-linking to obtain the heterojunction battery film; the thickness of the heterojunction battery film is 0.8 mm; the ultraviolet wavelength of the ultraviolet irradiation is 250 nm, and the irradiation time is 9 min.

[0036] Example 5

[0037] A heterojunction battery adhesive film is prepared from the following raw materials in parts by weight: 100 parts of EVA resin, 4 parts of 2,4-diphenyl-4-methyl-1-pentene, 3 parts of 2,4,6-trivinyl cycloboroxine, 1.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 5 parts of N-vinyl oxazolidinone, 5 parts of 1,3-bis(oxiranylmethyl)-5-(2-propylene)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1 part of 1,4-diamino-2,3-dicyanoanthraquinone, 2 parts of 3,3'-diamino-4,4'-difluorodiphenyl sulfone, 0.8 parts of photoinitiator, 0.8 parts of defoamer and 0.4 parts of antioxidant.

[0038] The antioxidant is antioxidant 1010; the defoamer is defoamer D6800; the photoinitiator is 2,4-dihydroxybenzophenone; the EVA resin is EVA provided by Taiwan Polymer Chemical Co., Ltd. UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28% and the melt flow rate is 25g / 10min.

[0039] A method for preparing the heterojunction battery film comprises the following steps: uniformly mixing the raw materials by weight, extruding the raw materials through a single-screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet irradiation cross-linking to obtain the heterojunction battery film; the thickness of the heterojunction battery film is 0.8 mm; the ultraviolet wavelength of the ultraviolet irradiation is 260 nm, and the irradiation time is 10 min.

[0040] Comparative Example 1

[0041] A heterojunction battery adhesive film and a preparation method thereof are basically the same as those in Example 1, except that 1,4-diamino-2,3-dicyanoanthraquinone and N-vinyloxazolidinone are not added.

[0042] Comparative Example 2

[0043] A heterojunction battery adhesive film and a preparation method thereof are basically the same as those in Example 1, except that 3,3'-diamino-4,4'-difluorodiphenyl sulfone and 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone are not added.

[0044] In order to further illustrate the beneficial technical effects of the heterojunction battery adhesive film involved in each embodiment of the present invention, the heterojunction battery adhesive film involved in Examples 1-5 and Comparative Examples 1-2 was subjected to relevant performance tests, and the test results are shown in Table 1. The test method refers to GB / T 29848-2018. Among them, the PCT aging performance (PCT 48h) is measured by the yellowing index before and after aging. The larger the value, the worse the PCT aging resistance; the high temperature and high humidity aging performance (DH1000h) is measured by the yellowing index before and after aging. The larger the value, the worse the high temperature and high humidity aging resistance.

[0045] It can be seen from the data in Table 1 that the heterojunction battery adhesive films involved in the embodiments of the present invention have better adhesion performance, high temperature and high humidity aging resistance and PCT aging resistance than the comparative example products, and better mechanical properties; the addition of 1,4-diamino-2,3-dicyanoanthraquinone, N-vinyl oxazolidinone, 3,3'-diamino-4,4'-difluorodiphenyl sulfone and 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone is beneficial to improving the above properties.

[0046] Table 1

[0047]

[0048] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A heterojunction battery adhesive film, characterized in that: The invention is prepared from the following raw materials by weight: 100 parts of EVA resin, 2-4 parts of 2,4-diphenyl-4-methyl-1-pentene, 1-3 parts of 2,4,6-trivinyl cycloboroxine, 0.8-1.5 parts of 3-(1,1-difluoro-2-propylene-1-yl)-2(1H)-quinoxalinone, 3-5 parts of N-vinyl oxazolidinone, 1,3-bis(oxiranylmethyl)-5 -(2-propenyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione 3-5 parts, 1,4-diamino-2,3-dicyanoanthraquinone 0.5-1 parts, 3,3'-diamino-4,4'-difluorodiphenyl sulfone 1-2 parts, photoinitiator 0.3-0.8 parts, defoamer 0.5-0.8 parts, antioxidant 0.1-0.4 parts; the EVA resin is EVA THENE® UE2828 type EVA resin, in which the mass percentage of vinyl acetate is 28% and the melt flow rate is 25g / 10min.

2. The heterojunction battery adhesive film according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010 and antioxidant 168.

3. The heterojunction battery adhesive film according to claim 1, characterized in that: The defoamer is at least one of defoamer AT-99 and defoamer D6800.

4. The heterojunction battery adhesive film according to claim 1, characterized in that: The photoinitiator is at least one of benzoin ethyl ether, benzoin isopropyl ether, diphenyl acetone, and 2,4-dihydroxybenzophenone.

5. A method for preparing a heterojunction battery adhesive film according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: uniformly mixing the raw materials by weight, extruding the raw materials through a single screw extruder to obtain a film, and then subjecting the cooled and shaped film to ultraviolet radiation cross-linking to obtain the heterojunction battery film.

6. The method for preparing the heterojunction battery adhesive film according to claim 5, characterized in that: The thickness of the heterojunction battery film is 0.5-1.2 mm.

7. The method for preparing the heterojunction battery adhesive film according to claim 5, characterized in that: The ultraviolet light wavelength of the ultraviolet light irradiation is 220-260nm, and the irradiation time is 5-10min.