A method for preparing zinc oxide array without mask

The zinc oxide array is prepared without masks by radio frequency magnetron sputtering and laser interference technology, which solves the problem of deposition and integration of zinc oxide nanostructures in the existing technology, and realizes high-quality, low-cost, and simple process nanostructure preparation. in a variety of electronic devices.

CN118308687BActive Publication Date: 2024-11-08NANJING UNIV OF POSTS & TELECOMM +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410736853.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-11-08
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

The prior art has problems in the preparation of zinc oxide nanostructures with difficult film uniformity, many defects, low deposition rate and the need for masks and photoresist when preparing zinc oxide nanostructures, making it difficult to achieve rapid processing on large areas and deposition and integration of high-quality nanostructures.

Method used

Using maskless preparation method, radio frequency magnetron sputtering combined with laser interference technology, multiple beams of laser interference form periodic spots on the substrate surface, promote the nucleation and deposition of zinc oxide nanoparticles, and form a high-quality zinc oxide array structure.

Benefits of technology

It realizes efficient preparation of zinc oxide nanostructures without development and etching and masks. It has simple process, low cost, short preparation period, flat film, low roughness, good crystallization quality, suitable for large-scale production and adjustable patterns Size and arrangement distribution, suitable for photoelectric display, transparent electrodes, photovoltaics and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118308687B_ABST
    Figure CN118308687B_ABST
Patent Text Reader

Abstract

The present application discloses a method for preparing a zinc oxide array without a mask, and belongs to the field of semiconductor process technology; the present application adopts a combination of magnetron sputtering and laser interference, and while depositing a thin film by magnetron sputtering, uses laser interference to form a patterned light intensity distribution on the substrate surface, so that each position of the substrate produces a thermal gradient distribution corresponding to the light intensity; the laser induces the growth of the surface morphology by changing the dynamics of surface adsorbed atoms; compared with the traditional method for preparing patterned array micro-nano structures, the present application has the advantages of simple process, low cost, short preparation cycle, no impurities, environmental friendliness, no need for photoresist, no mask, and adjustable pattern; the periodic patterned nanostructure prepared by the present invention can have luminescence, filtering, and bipolar transistor characteristics, and can be widely used in optoelectronic displays, transparent electrodes, photovoltaics, detectors, piezoelectric sensors, low-dimensional integrated device preparation and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of microelectronic manufacturing technology, and in particular to a method for preparing a zinc oxide array without a mask. Background Art

[0002] Patterned thin film is a technology that forms micro-nano structures on the surface of thin films. By controlling the shape, size and distribution of these structures, the thin film can be endowed with special optical, mechanical, electronic and other properties, playing an important role in optoelectronic display, photovoltaic, integrated circuit device preparation and other fields. Over the past few decades, nanotechnology has developed rapidly, and now there are many methods for preparing patterned nanostructures. Including electron beam lithography (EBL), focused ion beam lithography (FIB), nanoimprinting, self-assembled molecular synthesis, direct laser writing (DLW) and laser interferometry.

[0003] Among them, laser interference has been proven to be an attractive nanopatterning method due to its fast, economical and efficient characteristics. This method can create large-area, defect-free, one-dimensional, two-dimensional and even three-dimensional ordered nanostructures on various materials including semiconductors, metals and polymers. Traditional laser interference lithography technology involves photoresist and etching and has been widely used in the manufacture of semiconductor devices. Traditional laser interference technology uses the interference energy of light to form the characteristics of light field distribution with alternating light and dark. Through (specific beam combination method) the specific number of laser beams, interference angle and polarization direction, the intensity distribution of the interference field is controlled, and the patterned light field is recorded with photosensitive materials to prepare periodic structures, such as gratings, nanowires, quantum dot arrays, etc.

[0004] Thin film preparation is one of the important ways to achieve device miniaturization and integration. The preparation technology of zinc oxide thin film generally includes sol-gel, magnetron sputtering, chemical vapor deposition, pulsed laser deposition, atomic layer deposition and radio frequency magnetron sputtering. According to the category, it can be divided into physical method and chemical method. Electron beam evaporation, pulsed laser deposition and magnetron sputtering belong to physical methods; chemical vapor deposition, sol-gel and other technologies belong to chemical methods. The advantage of electron beam evaporation is that it can evaporate high melting point materials, the film growth rate is high, and the film purity is controllable, but the film uniformity is often uncontrollable and has many defects. The advantage of pulsed laser deposition technology is that the quality requirements of the target material are relatively low and the film has good adhesion to the substrate, but its limitation is that it cannot be mass-produced. Chemical vapor deposition is a thin film preparation technology with simple process and low cost, but its deposition rate is low. The sol-gel method is low-cost, the substrate shape is not limited, the equipment is simple, and it is suitable for large-scale production. The disadvantage of this method is that the film roughness is large and the film quality is relatively poor. Compared with other thin film preparation technologies, magnetron sputtering has many advantages. It can prepare high-quality, dense, low-roughness and high-adhesion thin film materials; it can control the crystal structure and orientation of the film; it can control the chemical composition and microstructure of the film, etc.

[0005] Among the existing patterned thin film preparation technologies, although EBL and FIB have high patterning resolution, they both require expensive instruments and photoresists. Microstructure manufacturing is based on pattern masks defined by photolithography. Usually, the process is long and time-consuming, making it unsuitable for large-area rapid processing of patterns. At the same time, if you want to accurately control the structure pattern morphology, you need to replace the mask. The precise assembly and integration of different nanostructures are still generally difficult. The uniformity of the film is difficult to control, and there are many defects. The film quality is not high, which is not suitable for large-area coating. The deposition rate is low, the uniformity of the film thickness is difficult to control, and the film quality is relatively low. Technical problems. The cost of nanoimprinting technology is significantly lower than that of photolithography technology. It is a typical top-down imaging method that can realize multi-scale structures on the target surface. However, this method is heavily dependent on PDMS molds and has limited accuracy.

[0006] Chinese patent application ZL202310507102.1 proposes a method of depositing a crystalline film by combining two laser beams with magnetron sputtering. Long-term irradiation is used to form a uniform thermal gradient on the substrate surface, thereby inducing the deposition of a high-quality film at the laser irradiation position. This method solves problems such as excessive film thickness, insufficient crystallinity, and low transmittance. However, the technical problem that the present invention needs to solve is different from that of the comparative document. The technical problem that this patent needs to solve is to use laser induction to achieve the deposition and integration of zinc oxide nanostructures on the film surface. Summary of the invention

[0007] A method for preparing a zinc oxide array without a mask, the specific steps of the preparation method are:

[0008] Step 1: Select a pure zinc oxide target with a purity of 99.999%, use a radio frequency magnetron sputtering source as the magnetron sputtering power source, and use a silicon substrate with a size of 10 mm × 10 mm;

[0009] Step 2: Place the pure zinc oxide target and silicon substrate in the corresponding positions in the vacuum chamber, with a target-substrate distance of 68 mm, and prepare the patterned structure by radio frequency magnetron sputtering. Set the initial temperature of the substrate to room temperature, and use high-purity Ar with a purity of 99.99% as the sputtering gas; the reference pressure in the vacuum chamber is 10 -4 When the pressure is in the Pa level, open the gas cylinder; the working pressure during sputtering is 0.15Pa. If the pressure is too low, the sputtering gas is difficult to ionize, and if the pressure is too high, the film quality will be poor; the sputtering power is 20-40W. If the power is lower than 20W, it will be difficult to perform glow discharge, and if the power is too high, the film roughness will increase; the sputtering time is 15-30min;

[0010] Step 3: During the sputtering process, a beam splitter is used to divide the laser source into multiple beams of coherent light and irradiate the substrate surface. The laser wavelength is 477nm, the power is 10mW, and the irradiation time is 15min-30min.

[0011] Step 4: By applying the principle of laser interference, a periodic patterned light spot is formed on the surface of the substrate; at these pattern positions, due to the characteristics of laser energy distribution, the film nucleation rate of the nanoparticles of the zinc oxide target in the light spot area is accelerated, ultimately leading to the formation of a protruding array structure.

[0012] As a preferred technical solution of the present invention: the size of the pure zinc oxide target is 48 mm in diameter and 3 mm in thickness.

[0013] As a preferred technical solution of the present invention: in the preparation of the patterned thin film by magnetron sputtering, the magnetron sputtering power source is a radio frequency AC power source with a frequency of 13.5 MHz.

[0014] As a preferred technical solution of the present invention: in the preparation of the patterned film, the reference pressure in the vacuum chamber is maintained at 10 -4 Pa level; the Ar flow rate is set to 20 sccm; when the pressure in the vacuum chamber is maintained at 4.5 Pa, the RF power is turned on.

[0015] As a preferred technical solution of the present invention: construct an optical path to achieve interference of multiple laser beams; use a beam splitter to split the laser into multiple beams, and concentrate the multiple coherent light beams on the substrate through reflection by a reflector to generate an interference pattern, thereby inducing the deposition of a zinc oxide array.

[0016] As a preferred technical solution of the present invention: when using a steady-state laser source Laser for irradiation, the six beams of light are reflected by the B1-B5 reflectors and finally converged on the substrate surface, thereby interfering to produce a periodically distributed light spot pattern, inducing rapid deposition of a zinc oxide array.

[0017] Beneficial effects of the present invention:

[0018] 1. The development of optical writing technology From contact / proximity exposure, projection exposure to the later developed laser direct writing technology, although it can achieve high-resolution pattern writing, all photolithography technologies require development and etching. The scheme of the present invention does not require development and etching, does not require a mask, and is not limited by the speed of light spot movement. Instead, it uses laser interference to induce the deposition of a patterned zinc oxide film at one time. It has the advantages of simple process, low cost, short preparation cycle, no impurities, no need for photolithography, and no mask.

[0019] 2. The processing of traditional patterned micro-nano structures will lead to the problem of uncontrollable particle size and arrangement distribution, while the zinc oxide pattern size obtained by multi-beam laser induced non-photolithography deposition can reach nanometer level and has luminescent properties.

[0020] 3. The distribution of the film surface structure can be adjusted by adjusting the spacing of the interference pattern; by adjusting the laser parameters, laser beam and polarization angle, the problem of pattern size and arrangement distribution can be solved. Therefore, adjusting the corresponding laser and light path parameters can change the deposition pattern structure without redesigning the layout and changing the mask.

[0021] 4. The film prepared by magnetron sputtering is flat, has low roughness, good crystal quality, fast deposition speed, and can be mass-produced.

[0022] 5. No mask or photoresist is required, the invention is environmentally friendly, has a short preparation cycle, a simple process, a low cost, rich and adjustable patterns, and is free of impurities. The zinc oxide patterned film prepared by the invention can have the characteristics of luminescence, filtering, and bipolar transistors, and can be widely used in optoelectronic display, transparent electrodes, photovoltaics, detectors, piezoelectric sensors, and low-dimensional integrated device preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the optical path of the laser interference system of the present application, including a double-beam and a triple-beam laser interference system, wherein (a) is an optical path diagram of the double-beam laser interference system, and (b) is an optical path diagram of the triple-beam laser interference system;

[0024] Figure 2 This is an AFM image of the zinc oxide array surface with double-beam laser interferometry and laser irradiation time of 15 min in this application;

[0025] Figure 3This is an AFM image of the zinc oxide array surface with three-beam laser interference and laser irradiation time of 30 min in this application. DETAILED DESCRIPTION

[0026] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. It should be noted that the words "front", "rear", "left", "right", "upper" and "lower" used in the following description refer to directions in the accompanying drawings, and the words "inner" and "outer" refer to directions toward or away from the geometric center of a specific component, respectively.

[0027] Example 1: This example proposes a method for preparing a zinc oxide array without a mask, and prepares a line-arranged dot pattern. The specific steps are:

[0028] Step 1: The target material is pure zinc oxide with a purity of 99.999%, the magnetron sputtering power source uses a radio frequency magnetron sputtering source, and the substrate is a P-type (100) crystal orientation silicon wafer with a size of 10 mm×10 mm;

[0029] Step 2: Place the zinc oxide target and substrate into the vacuum chamber. Before starting to prepare the pattern structure, the initial temperature of the substrate is set to room temperature, the target-substrate distance is 68 mm, and 99.99% pure Ar is used as the sputtering gas. Before coating, turn on the mechanical pump and molecular pump to pump the pressure in the vacuum chamber to 2.8×10 -4 After Pa, open the argon valve, set the gas flow rate to 20sccm on the control panel, turn on the RF power supply, set the sputtering power to 20W, and adjust the working gas pressure in the vacuum chamber to 0.15Pa, and then start pre-sputtering for 1 minute. The purpose of pre-sputtering is to remove impurities on the surface of the target material. After the pre-sputtering is completed, start thin film deposition sputtering;

[0030] Step 3: After the pre-sputtering operation is completed, set the incident angle and azimuth of the laser, and turn on the laser. The laser is divided into two beams by the beam splitter, such as Figure 1 As shown in (a); after being reflected by a reflector, it is finally focused on the center of the substrate surface. The laser wavelength is 477nm, the laser power is 10mW, the laser irradiation is 15min, and the magnetron sputtering is 15min. The two operations are carried out simultaneously.

[0031] Step 4: According to the principle of laser interference, a periodic spot pattern will be generated on the substrate surface. The target zinc oxide nanoparticles will deposit faster at the location of the spot, thus forming a periodic patterned structure with a linear point distribution. The period of the linear structure is about 1μm, and the pattern thickness is relatively low, about 8nm, such as Figure 2 shown.

[0032] Specific experimental parameters

[0033] Target material: Zinc oxide target with a purity of 99.999%, size is 48 mm in diameter and 3 mm in thickness.

[0034] Substrate: A silicon substrate with a crystal orientation of (1,0,0) and a size of 10 mm × 10 mm was used.

[0035] Target spacing: The target spacing is set to 68mm.

[0036] Sputtering gas: High-purity Ar gas with a purity of 99.999% and an argon gas flow rate of 20 sccm.

[0037] Irradiation time: 15 min. Selecting an appropriate irradiation time allows a sufficiently large energy gradient to be formed on the substrate surface. If the time is too short, such as less than 10 min, it is difficult to form a sufficient energy gradient on the substrate surface. If the time is too long, such as more than 30 min, the heat conduction of the substrate will easily cause the surface energy to be uniformly distributed, and it will be impossible to induce the zinc oxide nanoparticles to deposit into a high-resolution pattern.

[0038] Chamber pressure: The initial pressure in the vacuum chamber is 2.0×10 -4 Pa, and the pressure during sputtering was maintained at 0.15 Pa. The lattice was prepared under vacuum conditions to prevent the influence of impurities; the main reason for using 0.15 Pa is that when the working pressure is lower than 0.1 Pa, Ar is difficult to ionize and sputtering cannot be maintained; but when the working pressure is higher than 3.0 Pa, the quality of the deposited film is low, so the sputtering pressure is selected at 0.15 Pa as the working pressure.

[0039] Magnetron sputtering power supply: uses radio frequency discharge mode; mainly because the zinc oxide target material is a metal oxide semiconductor, its conductivity is not high, if a DC sputtering power supply is used, its efficiency is extremely low.

[0040] Laser parameter settings: The incident angle is set to , the azimuth is , , the laser wavelength is 477nm.

[0041] Example 2: This example proposes a method for preparing a zinc oxide array without a mask, and prepares a circular array structure. The specific steps are:

[0042] Step 1: Select a pure zinc oxide target with a purity of 99.999%, use a radio frequency magnetron sputtering source as the magnetron sputtering power source, and use a semiconductor or metal substrate with a size of 10 mm × 10 mm;

[0043] Step 2: Place the zinc oxide target and substrate into the vacuum chamber. Before starting to prepare the pattern structure, the initial temperature of the substrate is set to room temperature, the target-substrate distance is 68 mm, and 99.99% pure Ar is used as the sputtering gas. Before coating, turn on the mechanical pump and molecular pump to pump the pressure in the vacuum chamber to 2.8*10 -4 After Pa, open the argon valve, set the gas flow rate to 20sccm on the control panel, turn on the RF power supply, set the sputtering power to 20W, and adjust the working gas pressure in the vacuum chamber to 0.15Pa, and then start pre-sputtering for 1 minute. The purpose of pre-sputtering is to remove impurities on the surface of the target material. After the pre-sputtering is completed, start thin film deposition sputtering;

[0044] Step 3: When sputtering starts, turn on the laser, and the laser is divided into three beams by a beam splitter, such as Figure 1 As shown in (b); then it is reflected by a reflector and finally converged to the center of the substrate surface. The laser wavelength is 477nm, the laser power is 20mW, the laser irradiation is 30min, and the magnetron sputtering is 30min, and both are carried out simultaneously;

[0045] Step 4: According to the interference principle, a periodic pattern of light spots will be generated on the substrate surface. The zinc oxide nanoparticles will deposit faster at the location of the light spots, thus forming a structure similar to the pattern. The array obtained in this example has a small pattern structure thickness of about 8 nm under an atomic force microscope. The pattern distribution is as follows: Figure 3 shown.

[0046] Specific experimental parameters

[0047] Target material: Pure zinc oxide target with a purity of 99.999%, with a diameter of 48mm and a thickness of 3mm.

[0048] Substrate: A silicon substrate with a crystal orientation of (1,0,0) and a size of 10mm×10mm is used.

[0049] Target spacing: The target spacing is set to 68mm.

[0050] Sputtering gas: High-purity Ar gas with a purity of 99.999% and an argon gas flow rate of 20 sccm.

[0051] Irradiation time: 30 min. Select an appropriate irradiation time so that a sufficiently large energy gradient can be formed on the substrate surface. If the time is too short, such as less than 10 min, it is difficult to form a sufficient energy gradient on the substrate surface. If the time is too long, such as more than 30 min, the heat conduction of the substrate will easily cause the surface energy to be evenly distributed, and it will be impossible to induce the zinc oxide nanoparticles to deposit into a high-resolution pattern.

[0052] Chamber pressure: The initial pressure in the vacuum chamber is 1.5×10 -4Pa, and the pressure during sputtering was maintained at 0.15 Pa. The array was prepared under vacuum conditions to prevent the influence of impurities; 0.15 Pa was used mainly because, when the working pressure was lower than 0.1 Pa, Ar was difficult to ionize and sputtering could not be maintained; but when the working pressure was higher than 3.0 Pa, the quality of the deposited film was low, so the sputtering pressure was selected at 0.6 Pa as the working pressure.

[0053] Magnetron sputtering power supply: RF magnetron sputtering source is used. This is mainly because the zinc oxide target material is a polycrystalline semiconductor with low conductivity. If a DC sputtering power supply is used, its efficiency is extremely low.

[0054] Laser parameter settings: The incident angle is set to , the azimuth is , , , the laser wavelength is 477nm.

[0055] The technical means disclosed in the scheme of the present invention are not limited to the technical means disclosed in the above-mentioned implementation mode, but also include technical schemes composed of any combination of the above technical features.

Claims

1. A method for preparing a zinc oxide array without a mask, characterized in that: The specific steps of the preparation method are: Step 1: Select a pure zinc oxide target with a purity of 99.999%, use a radio frequency magnetron sputtering source as the magnetron sputtering power source, and use a silicon substrate with a size of 10 mm × 10 mm; Step 2: Place the pure zinc oxide target and silicon substrate into a vacuum chamber, and use laser interference induced magnetron sputtering to prepare a patterned film. Set the initial temperature of the silicon substrate to room temperature, the target-substrate distance to 68 mm, and the sputtering gas to 99.99% pure Ar. The working pressure during sputtering is 0.15 Pa, the sputtering power is 20-40 W, and the pre-sputtering time is 1 min. Step 3: While the thin film is being deposited, a steady-state laser source is used to generate coherent light through a beam splitter to irradiate the substrate surface. The laser wavelength is 477 nm, the power is 10-40 mW, and the irradiation time is 15 min-30 min. Step 4: By applying the principle of laser interference, a periodic patterned light spot is formed on the surface of the silicon substrate; at these pattern positions, due to the characteristics of the laser energy distribution, the film nucleation rate of the nanoparticles of the zinc oxide target in the light spot area is accelerated, ultimately leading to the formation of a protruding array structure.

2. The method for preparing a zinc oxide array without a mask according to claim 1, characterized in that: The size of the pure zinc oxide target in the preparation of patterned films is 48 mm in diameter and 3 mm in thickness.

3. The method for preparing a zinc oxide array without a mask according to claim 1, characterized in that: In the preparation of the patterned film, the magnetron sputtering power source is a radio frequency AC power source with a frequency of 13.5 MHz.

4. The method for preparing a zinc oxide array without a mask according to claim 1, characterized in that: The reference pressure in the vacuum chamber during the preparation of the patterned film is maintained at 10 -4 Pa level; the Ar flow rate is set to 20 sccm; when the pressure in the vacuum chamber is maintained at 4.5 Pa, the RF power is turned on.

5. The method for preparing a zinc oxide array without a mask according to claim 1, characterized in that: A beam splitter is used to split the laser beam into multiple beams, and multiple beams of coherent light are used to induce film growth; after being reflected by multiple mirrors, they are finally converged on the surface of the silicon substrate, thereby generating an interference pattern of multiple beams of coherent light, inducing the rapid deposition of a zinc oxide patterned film.

6. The method for preparing a zinc oxide array without a mask according to claim 5, characterized in that: A beam splitter is used to split the light beam into two or three beams; two laser beams interfere to form a linear array distribution, and three laser beams interfere to form a regular circular array.

7. The method for preparing a zinc oxide array without a mask according to claim 6, characterized in that: While using a steady-state laser source Laser for irradiation, multiple beams of light are reflected by the B1-B5 mirrors and finally converged on the surface of the silicon substrate, thereby interfering to produce a periodically distributed patterned light spot, inducing the rapid deposition of a zinc oxide patterned structure.