A heteroepitaxial growth method for low-dimensional tellurium dioxide crystals
By combining physical deposition and chemical deposition methods, the problems of low crystal quality and impurity contamination in low-dimensional tellurium dioxide crystal epitaxy are solved, high-quality nanosheet/nanowire preparation is achieved, and high-quality materials are provided for high-performance optoelectronic devices. .
Patent Information
- Application Number
- CN202410402261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-03
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-04-03
AI Technical Summary
It is difficult to achieve high-quality low-dimensional tellurium dioxide crystal epitaxy with existing technology. Conventional deposition technology has problems such as low crystal quality, difficulty in nucleation, and impurity contamination.
Using a method that combines physical deposition and chemical deposition, the tellurium film is prepared by magnetron sputtering and heated in a preset atmosphere. Vertical gaskets are used to adjust the distance between the substrate and the tellurium film and control the deposition temperature and atmosphere to achieve low-dimensional Heteroepitaxial growth of tellurium dioxide crystals.
The preparation of high-quality low-dimensional tellurium dioxide crystal nanosheets/nanowires was achieved, overcoming the problems of low crystal quality and impurity contamination, and providing material solutions for high-performance tellurium dioxide optoelectronic devices.
Smart Images

Figure CN118308786B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a low-dimensional material growth technology, and in particular to a heteroepitaxial growth method of a low-dimensional tellurium dioxide crystal. Background Art
[0002] Since the theoretical prediction, tellurium dioxide single crystal is a new type of low-dimensional semiconductor 1 , and has excellent electrical and optical properties, it has attracted widespread attention in the field of optoelectronic devices. The predicted electron mobility of low-dimensional tellurium dioxide is as high as 1000 cm 2 V -1 S -1 , hole mobility 9000cm 2 V -1 S -1 , and has a wide band gap of 3.2eV to 3.7eV, which complements the shortcomings of conventional two-dimensional semiconductors in the fields of low-dimensional power electronic devices and short-wave optoelectronic devices. The P-type band structure allows tellurium dioxide to form a PN junction with most of the widely studied N-type transition metal sulfide two-dimensional materials, which is used in two-dimensional LEDs, lasers, etc. It is expected to fill the lack of high-mobility P-type wide-bandgap two-dimensional materials and become a transformative material in the field of optoelectronics. However, so far, no experimental scheme has successfully prepared low-dimensional tellurium dioxide epitaxial crystals, and CMOS technology needs to rely on epitaxial thin films to manufacture optoelectronic devices. Due to the lack of high-quality thin film epitaxy technology, it is difficult to verify its predicted high performance.
[0003] The main methods for preparing tellurium dioxide thin films disclosed at present include magnetron sputtering. 2,3 , thermal evaporation 4,5 Sol-gel method 6 , each of which has advantages and disadvantages:
[0004] Magnetron sputtering is more controllable for the thickness of the film, but due to the limitation of post-annealing temperature, the film is often amorphous or polycrystalline, and there is a technical defect of incomplete oxidation.
[0005] The quality of crystals prepared by thermal evaporation is generally high, but they need to be deposited on a gold film. Gold as a catalyst will greatly enhance the preferred orientation of the crystals, thereby increasing the aspect ratio (greater than 1000) and making the tellurium dioxide crystals appear as elongated nanowires. On the other hand, a large amount of evaporation source at high temperature will lead to an uncontrollable deposition rate. Epitaxial films on amorphous substrates (quartz, SiO2 / Si, etc.) without gold film coverage are easily mixed with amorphous phases, resulting in impure crystal phases of the film.
[0006] The sol-gel method has lower requirements for substrates and equipment, but the film thickness of the coating is poorly controllable, and organic impurities are difficult to completely remove by relying solely on high-temperature annealing, which damages the quality of the film.
[0007] As for chemical vapor deposition, due to the low vapor pressure of Te source, nucleation is difficult, and there is no successful solution for depositing low-dimensional tellurium dioxide. There are only public reports on amorphous deposited films. 7 .
[0008] In summary, it is difficult to achieve the epitaxy of low-dimensional tellurium dioxide high-quality crystals using these existing conventional deposition techniques.
[0009] 1.Guo S, Zhu Z, Hu x, et al. ultrathin tellurium dioxide: emerging directbandgap semiconductor with high-mobility transport anisotropy[J]. Nanoscale, 2018, 10(18): 8397-8403.
[0010] 2.Siciliano T, Di Giulio M, Tepore M, et al.Room temperature NO2 sensingproperties of reactive sputtered TeO2 thin films[J].Sensors and ActuatorsB: Chemical, 2009, 137(2): 644-648.
[0011] 3. M, Walas M, Gapska A, et al.Structure and optical parameters of Eu doped tellurium oxide thin films prepared by reactive magnetron sputteringmethod[J]. Thin Solid Films, 2019, 691: 137592.
[0012] 4. Mahendar M, Krishna RNV, Chaudhary AK. Effect of the annealingtemperature on structural, morphological, and nonlinear optical properties of TeO2 thin films used for efficient THz generation [J]. Applied Optics, 2023, 62(10): 2394-2402.
[0013] 5.Yan C, Le BH, Kang D J. ultrasensitive single crystalline TeO2nanowire-based hydrogen gas sensors[J]. Journal of Materials Chemistry A, 2014, 2(15): 5394-5398.
[0014] 6. Bataliotti MD, Costa FB, Minussi FB, et al. Characterization of tellurium dioxide thin films obtained through the Pechini method [J]. Journal of Sol-Gel Science and Technology, 2022, 103(2): 378-385.
[0015] 7.Gupta PK, Sharma PP, Sharma A, et al. Electrochemical and antimicrobial activity of tellurium oxide nanoparticles[J]. Materials Science and Engineering: B, 2016, 211: 166-172. Summary of the invention
[0016] The present invention aims to provide a heteroepitaxial growth method of low-dimensional tellurium dioxide crystals to solve the problems existing in the above-mentioned prior art.
[0017] The heteroepitaxial growth method of a low-dimensional tellurium dioxide crystal described in the present invention sequentially performs physical deposition and chemical deposition;
[0018] The physical deposition: preparing a tellurium film on a substrate by magnetron sputtering;
[0019] The chemical deposition comprises: arranging a substrate above the tellurium film at a distance h; heating to a temperature T in a preset atmosphere and maintaining the temperature for a time t, so as to obtain the low-dimensional tellurium dioxide crystal on the side of the substrate facing the tellurium film.
[0020] The heteroepitaxial method of a low-dimensional tellurium dioxide crystal described in the present invention has the advantage of making the two technologies of physical deposition and chemical deposition complementary, overcoming the difficulties of difficult nucleation and low crystal quality, and realizing the epitaxial nanosheets / nanowires of low-dimensional tellurium dioxide crystals. A fixed-thickness amorphous tellurium film by magnetron sputtering is used as a vapor source to control the vapor pressure, while the deposition temperature and atmosphere are controlled by a tubular furnace. The distance between the epitaxial substrate and the tellurium film is fine-tuned by a vertical gasket, and the close distance between the source and the substrate greatly improves the nucleation efficiency. The size of the low-dimensional tellurium dioxide crystals epitaxially grown on an insulating substrate can reach several microns to tens of microns, without impurity contamination, and the crystal morphology can be controlled by substrate engineering. The material barriers for the preparation of high-performance tellurium dioxide optoelectronic devices are overcome. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is an optical microscope picture of a low-dimensional tellurium dioxide crystal produced on a mica substrate using the heteroepitaxial growth method described in the present invention.
[0022] Figure 2 This is an optical microscope picture of a low-dimensional tellurium dioxide crystal produced on a sapphire substrate using the heteroepitaxial method described in the present invention.
[0023] Figure 3 yes Figure 1 and Figure 2 Raman spectrum of the low-dimensional tellurium dioxide crystal shown.
[0024] Figure 4 yes Figure 1 and Figure 2 Grazing-incidence X-ray spectrum of the low-dimensional tellurium dioxide crystal shown.
[0025] Figure 5 yes Figure 1 and Figure 2 Photoluminescence spectrum of the low-dimensional tellurium dioxide crystal shown.
[0026] Figure 6 It is a schematic diagram of material arrangement during chemical deposition of the heteroepitaxial method described in the present invention.
[0027] Reference numerals: 10 - quartz boat, 11 - substrate, 12 - spacer, 13 - tellurium film. DETAILED DESCRIPTION
[0028] Embodiment 1
[0029] 1. Cleaning silicon / silicon dioxide wafers and mica wafers: Use acetone, isopropanol, and deionized water for ultrasonic cleaning three times each, each time for 5 minutes, and the ultrasonic power is 80 W. Among them, the oxide layer of the silicon / silicon dioxide wafer is selected to be 285nm and the size is selected to be 12mm×12mm, which is used as the substrate for preparing the tellurium film; the size of the mica wafer is selected to be 10mm×10mm, which is used as the substrate for growing low-dimensional tellurium dioxide crystals.
[0030] 2. The cleaned substrate is dried on a hot plate at 70°C for 10 minutes and set aside.
[0031] 3. Use 99.99% high-purity tellurium target as sputtering source to sputter tellurium film with a thickness of about 10nm to 20nm on the oxide layer of silicon / silicon dioxide wafer to obtain chemical vapor deposition source. The specific steps are as follows: After loading silicon / silicon dioxide wafer and target material, evacuate the magnetron sputtering chamber and maintain the vacuum degree to 8×10 -4 Pa. Argon gas was introduced as the ignition gas, the working pressure was set to 0.55 Pa, and a 20W DC source was used for sputtering; the argon flow rate during the sputtering process was set to 40 sccm, the substrate speed was 30 rad / min, and the sputtering time was 9min to 12min. After the sputtering was completed, the vacuum was released and the sample was taken out for use.
[0032] 4. Chemical vapor deposition: Specific sample loading is as follows Figure 6 As shown. The size of the quartz boat is 100mm×40mm×20mm, and the tellurium film obtained by the above magnetron sputtering is used as a trace controllable source. The tellurium film is placed upward in the quartz boat. Two small pieces of quartz are cut as gaskets. The size of the quartz sheet is 2mm×2mm and the thickness is 200μm. It is only placed in two directions along the wall of the quartz boat. The mica sheet is inverted on the tellurium film. The gasket makes the mica sheet suspended in the air. The suspension height is determined by the thickness of the gasket. This height has an important influence on the crystal size, because for a trace controllable source, the height of the gasket determines the saturated vapor pressure on the substrate surface.
[0033] 5. After the sample is correctly placed, start loading it into the quartz tube. The quartz tube used is equipped with a single-zone temperature-controlled heating furnace, a mechanical pump, and a gas circuit control. Open the quartz tube seal ring, and use the push rod to smoothly push the quartz boat to the center of the heating zone. Before heating the quartz boat, use a mechanical pump to remove the air in the quartz tube to reduce the vacuum to 1×10 -2 Torr. Then introduce a high-purity argon / air mixed atmosphere with a flow rate ratio of 9 / 1 to bring the pressure in the tube to normal pressure. Repeat the evacuation and then filling with the mixed gas 3-5 times to clean the quartz tube and remove excess air and water vapor in the tube.
[0034] 6. After cleaning, close the mechanical pump valve. Introduce argon / air mixed atmosphere at a constant speed, with the argon flow rate controlled at 90sccm and the air flow rate controlled at 10sccm, until the pressure in the tube reaches normal pressure and then close the air inlet valve.
[0035] 7. After the atmosphere is filled, start heating. The growth temperature used is 650℃, and the heating process is controlled to be 30-40min. After heating to the above specified temperature, keep the constant temperature for 15-20min to grow the crystal. After the growth stage is over, the quartz tube naturally cools to room temperature.
[0036] 8. Sampling. After cooling to room temperature, considering that Te vapor has certain toxicity, first evacuate the mixed gas in the quartz tube, then flush air into the quartz tube to clean it, repeat 2 to 3 times. Finally, open the sealing valve to take samples.
[0037] Embodiment 2
[0038] The difference from the first embodiment is that the key parameters are replaced according to the different substrate materials. In this embodiment, the substrate is a sapphire sheet. The corresponding key parameters are: the growth temperature is 600°C and the spacer height is 400μm.
[0039] The samples prepared according to the above-mentioned Example 1 and Example 2 were tested and analyzed respectively:
[0040] Taking into account the site adsorption in the early stage of nucleation, mica with an atomically flat surface is used as the substrate for epitaxial nanosheets, because monoclinic mica usually does not allow the nucleation to have a significant preferred orientation, and high flatness is conducive to reducing crystal defects. Figure 1 It is a nanosheet epitaxially grown on a mica substrate, with a size usually ranging from a few microns to tens of microns, and an aspect ratio of about 3:1. Smaller lattice mismatch often gives the epitaxial film a certain preferred orientation. In order to control the morphology of the crystal, a sapphire substrate with a lattice constant similar to that of tellurium dioxide is used for epitaxy to obtain nanowires, such as Figure 2 As shown, the length of the nanowire is about 20 microns, and the aspect ratio is about 20: 1. The tellurium dioxide crystals on the above insulating substrates are all van der Waals epitaxy, without impurity contamination, and the electrode pattern can be defined by conventional two-dimensional material transfer methods or lift-off on the substrate, thereby easily preparing high-performance field effect transistors or photodetectors or semiconductor heterojunctions and other optical and electronic devices.
[0041] The quality of the epitaxial crystals was characterized by Raman spectroscopy and grazing incidence X-ray spectroscopy (GIXRD). Figure 3 , Figure 4 First, Figure 3 Raman spectroscopy can identify that both nanowires and nanosheets have characteristic peaks that are completely consistent with tellurium dioxide crystals, including the typical 124cm -1and 151cm -1 TeO2 double peak. GIXRD is used to identify the type and quality of crystals. By comparing with the standard PDF card #78-1713, the crystal phase of tellurium dioxide is α-TeO2, rutile structure. Generally, the quality of crystals can be determined by the half-peak width of the low-order diffraction peaks on the GIXRD spectrum, that is, the diffraction peaks of the (110) and (102) crystal planes. Obviously, the two diffraction peaks are sharp and narrow, and the diffraction peaks of other crystal planes also have similar characteristics, indicating that the epitaxial crystals are single crystals and the crystal quality is comparable to other TeO2 thin film preparation literature. 2~6 Higher, especially compared to other epitaxial films grown by chemical vapor deposition 7 .
[0042] In order to evaluate the optical properties of the epitaxial crystals, the photoluminescence spectra (PL) were measured, such as Figure 5 . The PL spectrum is excited by 325nm laser. Both sample crystals can be excited and show consistent 380nm emission peak. Based on the principle of photoinduced transition, it can be calculated that the band gap of the two sample crystals is about 3.4eV, which is consistent with theoretical prediction.
[0043] For those skilled in the art, various other corresponding changes and deformations can be made according to the technical solutions and concepts described above, and all of these changes and deformations should fall within the protection scope of the claims of the present invention.
Claims
1. A heteroepitaxial method for low-dimensional tellurium dioxide crystals, characterized in that: Physical deposition and chemical deposition are carried out sequentially; The physical deposition: preparing a tellurium film on a substrate by magnetron sputtering; The chemical deposition comprises: arranging a substrate above the tellurium film at a distance h; heating to a temperature T in a preset atmosphere and maintaining the temperature at a constant temperature for a time t, and obtaining the low-dimensional tellurium dioxide crystal on the side of the substrate facing the tellurium film; the distance h between the tellurium film and the substrate is 200 μm to 400 μm; the preset atmosphere is an argon / air mixed atmosphere with a flow ratio of 9 / 1; the temperature T is 600°C to 650°C; and the time t is 15 min to 20 min.
2. The heteroepitaxial growth method of a low-dimensional tellurium dioxide crystal according to claim 1, characterized in that: The substrate is a silicon / silicon dioxide wafer.
3. The heteroepitaxial growth method of a low-dimensional tellurium dioxide crystal according to claim 1, characterized in that: The tellurium film has a thickness of 10 nm to 20 nm.
4. The heteroepitaxial growth method of a low-dimensional tellurium dioxide crystal according to claim 1, characterized in that: The substrate is made of mica or sapphire.
5. The heteroepitaxial growth method of a low-dimensional tellurium dioxide crystal according to claim 1, characterized in that: The distance between the tellurium film and the substrate is adjusted by a spacer.