A method for preparing silicon-oxygen negative electrode material by flux-assisted plasma method
By using a flux-assisted plasma method, the problems of high energy consumption and impurity generation in the preparation of silicon-oxygen anode materials in the existing technology have been solved, realizing the preparation of silicon-oxygen anode materials with low energy consumption and high purity, and improving the electrochemical performance of the materials.
Patent Information
- Application Number
- CN202410333206.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-21
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-21
AI Technical Summary
Existing technologies for preparing silicon-oxygen anode materials suffer from problems such as high equipment requirements, long reaction times, low production capacity, high costs, and impurity generation. Furthermore, conventional plasma methods require high voltage and current to ensure complete material vaporization.
The flux-assisted plasma method uses sodium salt or ammonium bicarbonate as a flux to perform a first plasma treatment and an optional second plasma treatment. The voltage and current are controlled within a low range, and the flux generates a greater enthalpy during ionization, ensuring complete vaporization of the material and removal of impurities.
The preparation of low-energy-consumption, high-purity silicon-oxygen anode materials has been achieved, improving the purity and electrochemical performance of the products, reducing energy consumption, and enhancing the discharge/charge specific capacity and first coulombic efficiency of the materials.
Smart Images

Figure CN118343769B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of silicon-oxygen materials, and in particular to a method for preparing silicon-oxygen negative electrode materials by a flux-assisted plasma method. Background Art
[0002] The current low energy density lithium-ion batteries are increasingly unable to meet people's needs, and the development of lithium-ion batteries with higher energy density has become a top priority. The theoretical specific capacity of the current mainstream graphite negative electrode material is only 372mAh·g -1 , which limits the improvement of lithium-ion battery energy density. Finding negative electrode materials with high specific capacity is one of the effective ways to improve the energy density of lithium-ion batteries. The theoretical capacity of silicon is as high as 4200mAh·g -1 , which is 10 times that of graphite anode. However, the volume expansion of silicon anode is as high as 300% during the process of lithium insertion and extraction, which can easily lead to the pulverization and shedding of materials and the repeated generation and destruction of SEI film, thus causing the performance of lithium-ion batteries to decline sharply. In contrast, silicon oxide (SiO x ) The negative electrode has a lower volume expansion (100-200%), but can provide a comparable specific capacity (>2000mAh·g -1 ), is currently expected to replace graphite and become one of the mainstream negative electrode materials in the future.
[0003] Current production of SiO x The mainstream processes for negative electrode materials are vacuum evaporation, hydrogen and carbon thermal reduction. These methods have high requirements for equipment, long reaction time, and cannot achieve continuous production, resulting in low production capacity and high cost. The carbon thermal reduction process has high requirements for temperature control and is very easy to generate SiC impurities. Hydrogen reduction of SiO2 has certain safety risks and cannot guarantee high-purity SiO x Plasma technology can effectively solve the shortcomings of the above processes. It not only has a rapid reaction but also has low requirements for raw materials, and can achieve efficient and fast production.
[0004] However, conventional plasma technology is used to prepare SiO x Usually a higher voltage and current (generally 20 to 50 kW) are required, otherwise the complete gasification of the material cannot be guaranteed, thus affecting the corresponding product. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing silicon-oxygen negative electrode materials by a flux-assisted plasma method. The method of the present invention can not only achieve lower energy consumption, but also ensure that the material is completely gasified to obtain a high-purity product.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing silicon-oxygen negative electrode materials by a flux-assisted plasma method, comprising the following steps: providing a mixture; the mixture comprises silicon powder, silicon dioxide and a flux; the flux is sodium salt or ammonium bicarbonate;
[0008] The mixed material is subjected to a first plasma treatment to obtain the silicon-oxygen negative electrode material; the working voltage of the first plasma treatment is 90 to 200 V, the current is 10 to 50 A, and the treatment time is 3 to 30 minutes.
[0009] Preferably, the sodium salt includes one or more of sodium silicate, sodium chloride, potassium sodium silicate, sodium borate, sodium bicarbonate and sodium thiosulfate.
[0010] Preferably, the mass ratio of the silicon powder to silicon dioxide is (1-1.5):1.
[0011] Preferably, the mass content of the flux in the mixture is 0.5-2%.
[0012] Preferably, the preparation of the mixed material comprises: mixing silicon powder, silicon dioxide and flux and ball-milling them, and sieving the obtained ball-milled material to obtain the mixed material.
[0013] Preferably, the screening is through a 100-300 mesh sieve.
[0014] Preferably, after the first plasma treatment, the method further comprises subjecting the obtained first plasma treatment product to a second plasma treatment; the working voltage of the second plasma treatment is 90 to 200 V, the current is 10 to 50 A, and the treatment time is 3 to 30 min.
[0015] Preferably, the carrier gases used in the first plasma treatment and the second plasma treatment are independently Ar and / or H2.
[0016] Preferably, after the second plasma treatment, the obtained product is further cooled, collected, washed and dried in sequence.
[0017] The present invention provides a method for preparing silicon-oxygen negative electrode materials by a flux-assisted plasma method, comprising the following steps: providing a mixture; the mixture comprises silicon powder, silicon dioxide and a flux; the flux is a sodium salt or ammonium bicarbonate; the mixture is subjected to a first plasma treatment to obtain the silicon-oxygen negative electrode material; the working voltage of the first plasma treatment is 90 to 200 V, the current is 10 to 50 A, and the treatment time is 3 to 30 min. The present invention can generate greater heat enthalpy during the ionization process by adding a flux, thereby accelerating the gasification of the solid, so that the material can be completely gasified at a lower power to obtain a high-purity product, thereby reducing energy consumption.
[0018] Furthermore, the present invention can further completely react the substances in the product of the first plasma treatment by performing a secondary plasma treatment on the product, and can remove impurities therein to obtain SiO with higher purity. x . BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a SEM image of the silicon-oxygen negative electrode material prepared in Example 1;
[0020] Figure 2 XRD pattern (a) and charge-discharge curve (b) of the silicon-oxygen negative electrode material prepared in Example 1;
[0021] Figure 3 This is a cycle curve diagram of the silicon-oxygen negative electrode material prepared in Example 1. DETAILED DESCRIPTION
[0022] The present invention provides a method for preparing silicon-oxygen negative electrode materials by a flux-assisted plasma method, comprising the following steps: providing a mixture; the mixture comprises silicon powder, silicon dioxide and a flux; the flux is sodium salt or ammonium bicarbonate;
[0023] The mixed material is subjected to a first plasma treatment to obtain the silicon-oxygen negative electrode material; the working voltage of the first plasma treatment is 90 to 200 V, the current is 10 to 50 A, and the treatment time is 3 to 30 minutes.
[0024] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0025] The invention first provides a mixed material; the mixed material comprises silicon powder, silicon dioxide and flux.
[0026] In the present invention, the flux is a sodium salt or ammonium bicarbonate, and the sodium salt preferably includes one or more of sodium silicate, sodium chloride, potassium sodium silicate, sodium borate, sodium bicarbonate and sodium thiosulfate.
[0027] In the present invention, the purity of the silicon powder is preferably above 99%; the silicon powder is preferably obtained by grinding photovoltaic scraps.
[0028] The present invention has no special requirements on the source of the silicon dioxide, and any silicon dioxide known in the art can be used, such as high-purity silicon dioxide (purity> 99.9%) and quartz sand (considered to be large-particle silicon dioxide).
[0029] In the present invention, the mass ratio of the silicon powder to silicon dioxide is preferably (1-1.5):1, and more preferably (1.1-1.2):1.
[0030] In the present invention, the mass content of the flux in the mixture is preferably 0.5-2%, more preferably 0.8-1.6%, and further preferably 1-1.2%.
[0031] In the present invention, the preparation of the mixed material preferably comprises: mixing silicon powder, silicon dioxide and flux and ball-milling them, and sieving the obtained ball-milled material to obtain the mixed material.
[0032] In the present invention, before the mixed ball milling, the particle size of the silicon powder is preferably 3-5 μm, the particle size of the silicon dioxide is preferably 300-500 nm, and the particle size of the quartz sand is preferably 150-200 μm. The present invention has no special requirements for the conditions of the mixed ball milling, as long as the materials can be mixed evenly. In an embodiment of the present invention, the rotation speed of the mixed ball milling is 800 r / min and the time is 30 min.
[0033] In the present invention, the screening is preferably through a 100-300 mesh sieve; the present invention preferably uses a vibrating sieving machine for screening.
[0034] After obtaining the mixed material, the present invention performs a first plasma treatment on the mixed material.
[0035] In the present invention, the working voltage of the first plasma treatment is 90-200V, preferably 100-180V, more preferably 120-160V; the current of the first plasma treatment is 10-50A, preferably 20-40A, more preferably 25-35A; the time of the first plasma treatment is 3-30min, preferably 10-25min, more preferably 15-20min. The present invention can generate greater heat enthalpy in the ionization process by adding flux, thereby accelerating the gasification of solids. Therefore, the material can be completely gasified to obtain a high-purity product at a lower power, thereby reducing energy consumption.
[0036] In the present invention, the carrier gas used for the first plasma treatment is preferably Ar and / or H2. When the carrier gas is Ar and H2, the volume ratio of Ar to H2 is preferably 1:(0.1-1). The present invention has no special requirements on the flow rate of the carrier gas, and any carrier gas flow rate known in the art can be used. In an embodiment of the present invention, the flow rate of the carrier gas is 10 L / min.
[0037] In the first plasma treatment process of the present invention, the following reaction occurs: Si+SiO2→SiO x .
[0038] After completing the first plasma treatment, the present invention preferably cools, collects, washes and dries the obtained treatment product to obtain a first powder.
[0039] In the present invention, the washing is preferably deionized water washing, or washing with a mixed solution of deionized water and alcohol; the alcohol is preferably methanol or ethanol. In the present invention, when washing with a mixed solution of deionized water and alcohol, the volume ratio of deionized water to alcohol is preferably 1:(0.5 - 1). During the washing process of the present invention, the flux dissolves in water and is thus removed. In the present invention, the drying is preferably vacuum drying.
[0040] In the present invention, when the second plasma treatment is not carried out, the first powder obtained in the present invention is the silicon-oxygen anode material. In the present invention, when the second plasma treatment is carried out, the present invention preferably subjects the first powder to the second plasma treatment.
[0041] In the present invention, the conditions of the second plasma treatment are applicable to the first plasma treatment and will not be elaborated here. Through the second plasma treatment of the present invention, the substances in the first powder can further fully react, and impurities therein can be removed to obtain SiO with higher purity. x 。
[0042] After completing the second plasma treatment, the present invention preferably cools, collects, washes, and dries the obtained product in sequence to obtain the silicon-oxygen anode material. In the present invention, the cooling, collection, washing, and drying are the same as above and will not be elaborated here.
[0043] In the present invention, the plasma equipment used for the first plasma treatment and the second plasma treatment preferably is the preparation system for spherical micro-nano powders in the patent application with the application number of "202311326816.9" and the invention title of "A Preparation System and Preparation Method for Spherical Micro-Nano Powders".
[0044] The silicon-oxygen material prepared by the method of the present invention shows amorphous diffuse peaks in XRD, so the obtained product is amorphous. Through oxygen content test calculation, its component is SiO x (0.8 < x < 1.2). The obtained product is assembled into a coin-type half-cell, and its first discharge capacity / charge capacity is at most 2187 / 1326 mAh·g -1 respectively, and the corresponding first Coulomb efficiency is 60.63%.
[0045] The SiO x material prepared by the present invention has high sphericity, less aggregation, and uniform dispersion, and its diameter distribution is in the range of 5 - 300 nm.
[0046] The following combines examples to elaborate in detail on the method for preparing a silicon-oxygen anode material by a flux-assisted plasma method provided by the present invention, but they should not be construed as limiting the protection scope of the present invention.
[0047] Example 1
[0048] Photovoltaic silicon powder (3-5 μm) and high-purity silicon dioxide (300-500 nm) were mixed in a ratio of 1.25:1, and 1% sodium silicate of the total mass of the raw materials was added as a flux. The ball milling was carried out at a ball-to-material ratio of 1.5:1, with a rotation speed of 800 r / min and a time of 30 min. Then, a 100-mesh vibrating sieve was used to sieve the fine powder. The fine powder was transferred to the feeder of the plasma equipment, with argon as the carrier gas and a flow rate of 10 L / min. The current of the plasma equipment was 50 A, the voltage was 130 V, and the processing time was 10 min. The mixed solution of deionized water and methanol (the volume ratio of deionized water and methanol was 1:1) was used for washing and vacuum drying to obtain SiO x Negative electrode material, wherein x=0.9.
[0049] SiO prepared in Example 1 x The morphology of the negative electrode material is uniformly spherical, with a diameter distribution of 50 to 100 nm (such as Figure 1 shown).
[0050] The XRD characterization results are shown in Figure 2 Middle (a). Figure 2 As can be seen from (a), the silicon-oxygen material prepared by the method of the present invention exhibits an amorphous dispersion peak in XRD, so the obtained product is amorphous. In addition, no other phases are observed in the XRD spectrum, indicating that the obtained SiO x The negative electrode material is of high purity.
[0051] The electrodes were prepared and the charge and discharge tests were carried out. Specifically, the active material: binder: conductive agent were mixed in a mass ratio of 8:1:1. The active material was SiO x The negative electrode material, the binder is polyacrylic acid, the conductive agent is acetylene black, and an appropriate amount of deionized water is added. The slurry is obtained by high-speed stirring at a speed of 1500r / min. The obtained slurry is coated on a copper foil with a thickness of 200μm, and then transferred to a blast oven for drying for 8 hours to obtain an electrode; metallic lithium is used as a counter electrode, PP is used as a diaphragm, and the electrolyte is 1M LiPF6 dissolved in EC:DEC:EMC (1:1:1 volume ratio). The test current is 100mA·g -1 , the voltage range is 0.01~1.5V, the test results are shown in Figure 2 (b) The results show that the first discharge / charge capacity is 2146 / 1244 mAh g -1 , the first coulombic efficiency is 58%.
[0052] Figure 3 is a cycle curve diagram of the silicon-oxygen negative electrode material prepared in Example 1, Figure 3It can be seen that the silicon-oxygen negative electrode material prepared by the present invention has good cycle stability. After 20 cycles, its discharge / charge specific capacity and coulombic efficiency remain basically unchanged.
[0053] Example 2
[0054] Photovoltaic silicon powder was mixed with high-purity silicon dioxide and quartz sand in a ratio of 1.25:0.5:0.5, and 1% sodium chloride was added. The ball milling was carried out at a ball-to-material ratio of 1.5:1, with a rotation speed of 800r / min and a time of 30min. Then, a 100-mesh vibrating sieve was used to sieve the fine powder. The powder was transferred to the plasma equipment, with argon as the carrier gas, a flow rate of 10L / min, a current of 50A, a voltage of 130V, and a processing time of 10min. The powder was washed with a mixed solution of deionized water and methanol (the volume ratio of deionized water to methanol was 1:0.5) and vacuum dried to obtain SiO x Negative electrode material, wherein x=1.12.
[0055] Example 2 SiO x The morphology of the negative electrode material is uniformly spherical, with a diameter distribution of 5 to 50 nm, and the first discharge / charge specific capacity is 1936 / 813 mAh g -1 , the first coulombic efficiency is 42%.
[0056] Example 3
[0057] The difference from Example 2 is that 1% sodium borate is added to 1% sodium chloride, and the other processes and conditions are the same to obtain SiO x Negative electrode material, wherein x=0.95.
[0058] The prepared material is spherical and directly distributed in 20-50nm, with an initial discharge / charge capacity of 2021 / 1071mAh·g -1 , the first Coulombic efficiency is 53%.
[0059] Example 4
[0060] Photovoltaic silicon powder and quartz sand were mixed in a ratio of 1.5:1, and sodium silicate, potassium sodium silicate and sodium borate were added as flux (mass ratio was 1:1:1; the amount of flux added was 1%) for ball milling and mixing, sieved through 200 mesh, and then transferred to a plasma device with a current of 10A, a voltage of 110V, and a treatment time of 30min. The mixture was washed and dried with a mixture of ethanol and deionized water (the volume ratio of deionized water to ethanol was 1:0.5) to obtain SiO x Negative electrode material, wherein x=0.85.
[0061] The material is spherical in shape with a diameter ranging from 60 to 150 nm. The first discharge / charge specific capacity is 2187 / 1326 mAh g -1 , the first coulombic efficiency is 60.63%.
[0062] Example 5
[0063] The sample prepared in Example 2 was subjected to secondary plasma treatment under the same treatment conditions as in Example 2 to obtain SiO x Negative electrode material, wherein x=0.8.
[0064] The material is spherical in shape with a diameter ranging from 50 to 300 nm. The first discharge / charge specific capacity is 2259 / 1468 mAh g -1 , the first coulombic efficiency is 64.98%.
[0065] It can be seen from the results of Example 5 and Comparative Example 2 that secondary plasma treatment can further improve the purity of the silicon-oxygen negative electrode material, thereby improving its discharge / charge specific capacity and first coulombic efficiency.
[0066] Comparative Example 1
[0067] The only difference from Example 1 is that no flux is added, and SiO x Negative electrode material, wherein x=1.05.
[0068] Comparative Example 1 SiO x The morphology of the negative electrode material is uniformly spherical, with a diameter distribution of 100-300nm, and the first discharge / charge specific capacity is 1450 / 580mAh·g -1 , the first coulombic efficiency is 40%.
[0069] It can be seen from the results of Example 1 and Comparative Example 1 that the present invention can generate greater thermal enthalpy at the same power by adding flux, thereby promoting more complete gasification of the material to obtain high-purity silicon oxide negative electrode material, which is beneficial to improving its discharge / charge specific capacity and first coulombic efficiency.
[0070] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a silicon-oxygen negative electrode material by a flux-assisted plasma method, comprising the following steps: Providing a mixture; the mixture comprises silicon powder, silicon dioxide and a flux; the flux is sodium salt or ammonium bicarbonate; The mixed material is subjected to a first plasma treatment to obtain the silicon-oxygen negative electrode material; the working voltage of the first plasma treatment is 90 to 200 V, the current is 10 to 50 A, and the treatment time is 3 to 30 minutes.
2. The method according to claim 1, characterized in that The sodium salt includes one or more of sodium silicate, sodium chloride, potassium sodium silicate, sodium borate, sodium bicarbonate and sodium thiosulfate.
3. The method according to claim 1, characterized in that The mass ratio of the silicon powder to silicon dioxide is (1-1.5):
1.
4. The method according to any one of claims 1 to 3, characterized in that: The mass content of the flux in the mixture is 0.5-2%.
5. The method according to claim 1, characterized in that The preparation of the mixed material comprises: mixing silicon powder, silicon dioxide and flux and ball-milling them, and sieving the obtained ball-milled material to obtain the mixed material.
6. The method according to claim 5, characterized in that The sieving is through a 100-300 mesh sieve.
7. The method according to claim 1, characterized in that After the first plasma treatment, the method further includes subjecting the obtained first plasma treatment product to a second plasma treatment; the working voltage of the second plasma treatment is 90 to 200 V, the current is 10 to 50 A, and the treatment time is 3 to 30 minutes.
8. The method according to claim 7, characterized in that The carrier gases used in the first plasma treatment and the second plasma treatment are independently Ar and / or H2.
9. The method according to claim 7, characterized in that: After the second plasma treatment, the method further includes sequentially cooling, collecting, washing and drying the obtained product.
Citation Information
Patent Citations
Preparation system and preparation method of spherical micro-nano powder
CN117398949A
Method for recovering rare earth metals in fly ash by utilizing plasma
CN110527839A
Preparation method of nano silicon monoxide powder
CN114349011A
Method for preparing silicon monoxide by adding fluxing agent
CN116161667A
METHOD FOR PRODUCING SiOx (x<1)