A production process for high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material

By using high-temperature binder technology of compounded ceramic particles and reinforced particles in alloy steel materials, a high-strength ceramic preform is formed and closely combined with the alloy steel liquid, the problem of poor bonding of ceramic particles and metal liquid is solved, and the problem of significant improvement is improved The mechanical properties and wear resistance of the material have been extended, and the service life is expanded.

CN118344158BActive Publication Date: 2024-11-12SHANDONG XINGHE SPECIAL MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410462081.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-11-12
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

The poor interface bonding between ceramic particles and metal liquid in existing alloy steel materials leads to poor mechanical properties and short service life, which limits its application scenarios.

Method used

The high-temperature binder process of compounded ceramic particles and reinforced particles is used to form a high-strength, hardness and wear-resistant ceramic preform through the treatment of specific temperature and pressure, and cast with the alloy steel liquid metal to ensure close bond.

Benefits of technology

It improves the mechanical properties, hardness and wear resistance of alloy steel-based melt-cast ceramic materials, extends the service life and expands its application areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004796117570000041
    Figure BDA0004796117570000041
Patent Text Reader

Abstract

The present invention discloses a production process of a high-strength integrated alloy steel-based melt-cast ceramic wear-resistant material, which relates to the technical field of alloy ceramic wear-resistant materials, and comprises the following steps: preparing raw materials of a preform, comprising ≤83wt% of composite ceramic particles, 15-25wt% of composite reinforcing particles, and 2-3.5wt% of a binder, fully mixing the binder with the composite particle material, filling the premix into a mold, warm-pressing to obtain a ceramic preform, placing the ceramic preform in a casting mold, vacuumizing after closing the mold, then casting the alloy steel metal liquid infiltration preform, sintering and tempering the material to obtain a finished product. The alloy steel-based melt-cast ceramic wear-resistant material of the present invention solves the problem of poor bonding between raw material components. The new alloy ceramic wear-resistant material has excellent mechanical strength, hardness and wear resistance, long service life, and a wide range of application fields and occasions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy ceramic wear-resistant materials, and in particular to a production process of a high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material. Background Art

[0002] Metal materials are important engineering materials. Among metal materials, 90% are steel. Steel materials have the characteristics of low price, abundant resources, superior performance and easy large-scale production, and have been widely used. How to improve the performance of alloy steel materials has also become the research goal of many scholars at home and abroad. One of the important research directions is to prepare reinforcing particles and compound them into alloy steel materials to form alloy steel-based composite materials. There are existing preforms in alloy steel materials as reinforcing materials on the market to improve the service life of composite materials, and there are also hard ceramic micropowders such as WC, TiC, VC and other densified micropowders introduced into alloy steel materials to enhance the properties of materials. However, there are some problems with the alloy steel ceramic reinforcements obtained by the current preparation method. For example, the interface bonding of the components in the material is not good, resulting in the inability of the internal materials to adapt and complete the bonding reaction during casting and filling, resulting in poor mechanical properties of the obtained materials, which are specifically manifested in low mechanical strength, wear resistance and hardness values, which in turn limits the application scenarios of alloy ceramic composite materials and the problem of short material service life. Summary of the invention

[0003] In view of the problems existing in the prior art, the object of the present invention is to provide a production process of a high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material, which specifically comprises the following steps:

[0004] Step 1: Obtain raw materials for preparing a preform, including the following raw materials in percentage by weight:

[0005] Composite ceramic particles ≤ 83wt%;

[0006] Compound reinforcement particles 15-25wt%;

[0007] Binder 2-3.5wt%;

[0008] The composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles; the composite reinforcement particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder and molybdenum powder;

[0009] Step 2: Clean the surfaces of the obtained silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles, yttrium oxide ceramic particles and reinforcement particles, dry them thoroughly and mix them for later use;

[0010] Step 3: Add the binder to the composite granular material of step 2, first stir and mix at room temperature for 15 minutes; then heat to 180-200°C at a rate of 120°C / h, stir and mix for 12 minutes; then heat to 340-360°C at a rate of 100°C / h, stir and mix for 10 minutes; then heat to 520-540°C at a rate of 80°C / h, stir and mix for 8 minutes; finally heat to 700-720°C at a rate of 60°C / h, stir and mix for 5 minutes to obtain a premix;

[0011] Step 4: Fill the premix into the mold, warm press molding, the heating temperature is 80-100°C, the pressing pressure is 35MPa, and after molding and demolding, it is first allowed to stand at room temperature for 12 hours, and then put into the oven for heating at 60-80°C for 3 hours, and then heated to 150-160°C at a rate of 5°C / min for 2 hours, and then slowly cooled and taken out for 24 hours to obtain a ceramic preform;

[0012] Step 5: placing the ceramic preform in a casting mold, and preheating the ceramic preform and the casting mold to 860-880°C, vacuumizing the mold after closing, and then casting the alloy steel molten metal to infiltrate the preform. The casting temperature of the alloy steel molten metal is 1580°C ± 5°C. After the casting is completed, a semi-finished alloy steel-based fused-cast ceramic wear-resistant material is obtained;

[0013] Step 6: Sinter the semi-finished material at 1120-1140°C in an inert gas atmosphere for 3.5 hours with a sintering pressure of 50MPa, take it out and air-cool it, then keep it at 960-980°C for 2.5 hours and then air-cool it, and finally keep it at 335-355°C for 2 hours to obtain the finished alloy steel-based melt-cast ceramic wear-resistant material.

[0014] Furthermore, the particle size of the composite ceramic particles ranges from 2 to 5 mm.

[0015] Furthermore, the composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles in a mass ratio of 2:2:1:1.

[0016] Furthermore, in the composite ceramic particles, the particle size of the silicon nitride ceramic particles is 4-5 mm, the particle size of the zirconium oxide ceramic particles is 2.5-3.5 mm, the particle size of the tungsten carbide ceramic particles is 3-4.5 mm, and the particle size of the yttrium oxide ceramic particles is 2-3 mm.

[0017] Furthermore, the particle size of the composite reinforced particles ranges from 0.5 to 2 mm.

[0018] Furthermore, the composite reinforced particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder and molybdenum powder in a mass ratio of 6:2:1:1:1.

[0019] Preferably, the adhesive is HR-8767A alumina high temperature adhesive, which is an inorganic ceramic component, can withstand high temperatures of 1730°C, has strong bonding with metals and ceramics, and is resistant to aging, acid and alkali.

[0020] Furthermore, the volume fraction of the ceramic preform in the alloy steel-based fused-cast ceramic wear-resistant material is 30.5 vt%.

[0021] Furthermore, the alloy steel molten metal contains the following chemical components in mass percentage: carbon 0.35%, silicon 0.70%, manganese 17.8%, chromium 12.5%, vanadium 1.2%, niobium 0.26%, titanium 0.15%, nitrogen 0.3%, sulfur ≤0.03%, phosphorus ≤0.03%, and the remainder is Fe and unavoidable impurities, and the impurity content is ≤0.15%.

[0022] Compared with the prior art, the alloy steel-based fused-cast ceramic wear-resistant material production process of the embodiment of the present application has at least the following beneficial effects: the alloy steel-based fused-cast ceramic wear-resistant material of the embodiment of the present application is prepared by composite ceramic particles, composite reinforcing particles, high temperature resistant binder (HR-8767A alumina high temperature glue) and alloy steel molten metal and adopts a specific production process. Ceramic particles and reinforcing particles of different materials and particle size ranges are used in the process. On the one hand, a skeleton with high strength, high hardness, high wear resistance and stability is formed by mixing and reacting with the high temperature binder. On the other hand, a large number of fine pore channels exist in the formed skeleton and are connected, which is beneficial to the later stage of the process. The alloy steel molten metal can be cast and infiltrated into the interior of the preform during casting, thereby realizing the tightness of the combination of the ceramic preform and the alloy steel molten metal. In addition, due to the alloy steel molten metal The metal liquid can be cast and infiltrated into the ceramsite preform from multiple directions and angles, ensuring a good interface bonding between the ceramic preform and the alloy steel metal liquid in the matrix material, thereby forming a unique reinforcement, hardening, wear-enhancing and toughening structure, and improving the comprehensive mechanical properties of the wear-resistant material. The ceramic preform and the alloy steel metal liquid are integrated not only to improve the mechanical strength of the single ceramic composite material (ceramic preform), but also to effectively improve the tendency of brittle cracking when the matrix is ​​strained, thereby improving the impact toughness of the material. Moreover, the alloy steel-based fused-cast ceramic wear-resistant material prepared in the embodiment of the present application exhibits good hardness and wear resistance, and can effectively resist the cutting and plowing action of abrasives. Therefore, from the perspective of performance effect, the alloy steel-based fused-cast ceramic wear-resistant material described in the embodiment of the present application has good market potential and a wide range of application fields and occasions. DETAILED DESCRIPTION

[0023] The specific implementation modes of the present invention are further described below in conjunction with examples. The following examples are only used to more clearly illustrate the technical solutions of the present invention, and are not intended to limit the protection scope of the present invention.

[0024] Example 1

[0025] Example 1 of the present application discloses a production process of a high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material, comprising the following steps:

[0026] Step 1: Obtain raw materials for preparing a preform, including the following raw materials in percentage by weight:

[0027] Composite ceramic particles 83wt%;

[0028] Compound reinforcement particles 15wt%;

[0029] Binder 2wt%;

[0030] The particle size of the composite ceramic particles is in the range of 2 to 5 mm, and the composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles in a mass ratio of 2:2:1:1.

[0031] In this embodiment, the particle size of the silicon nitride ceramic particles in the composite ceramic particles is 4-5 mm, the particle size of the zirconium oxide ceramic particles is 2.5-3.5 mm, the particle size of the tungsten carbide ceramic particles is 3-4.5 mm, and the particle size of the yttrium oxide ceramic particles is 2-3 mm.

[0032] In this embodiment, the particle size of the composite reinforcement particles ranges from 0.5 to 2 mm, and the composite reinforcement particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder, and molybdenum powder in a mass ratio of 6:2:1:1:1;

[0033] In some embodiments of the present application, the adhesive is a high temperature resistant adhesive, the brand name is HR-8767A alumina high temperature adhesive (purchased from Dongguan Huirui Adhesive Co., Ltd.), which is composed of agent A and agent B. It should be noted that this adhesive is an inorganic ceramic component, which can withstand high temperatures of 1730°C, has strong bonding with metals and ceramics, and is resistant to aging and acid and alkali. The specific parameters are shown in Table 1 below:

[0034] Table 1: HR-8767A Alumina High Temperature Adhesive Product Parameters

[0035]

[0036] Step 2: Clean the surfaces of the obtained silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles, yttrium oxide ceramic particles and reinforcement particles, dry them thoroughly and mix them for later use;

[0037] Step 3: Use an electronic weighing tool to correctly mix the binder according to the instructions in Table 1, add the binder to the composite granular material in step 2, first stir and mix at room temperature for 15 minutes; then heat to 180°C at a rate of 120°C / h, stir and mix for 12 minutes; then heat to 340°C at a rate of 100°C / h, stir and mix for 10 minutes; then heat to 520°C at a rate of 80°C / h, stir and mix for 8 minutes; finally heat to 700°C at a rate of 60°C / h, stir and mix for 5 minutes to obtain a premix;

[0038] Step 4: Fill the premix into a mold of a certain shape, and perform warm pressing molding. The heating temperature is 80°C and the pressing pressure is 35MPa. After molding and demolding, let it stand at room temperature for 12 hours, put it into an oven and heat it at 60°C for 3 hours, then heat it to 150°C at a rate of 5°C / min and keep it warm for 2 hours. After slowly cooling, take it out and place it for 24 hours to obtain a ceramic preform.

[0039] Step 5: placing the ceramic preform in the mold, and preheating the ceramic preform and the mold to 860°C, vacuuming after the mold is closed, and then casting the alloy steel molten metal to infiltrate the preform. The casting temperature of the alloy steel molten metal is 1580°C ± 5°C. After the casting is completed, a semi-finished alloy steel-based fused-cast ceramic wear-resistant material is obtained;

[0040] The volume fraction of the ceramic preform in the alloy steel-based fused-cast ceramic wear-resistant material is 30.5vt%. In this embodiment, the alloy steel molten metal contains the following chemical components in percentage by mass:

[0041] Carbon 0.35%, silicon 0.70%, manganese 17.8%, chromium 12.5%, vanadium 1.2%, niobium 0.26%, titanium 0.15%, nitrogen 0.3%, sulfur ≤0.03%, phosphorus ≤0.03%, the balance is Fe and unavoidable impurities, impurity content ≤0.15%.

[0042] Step 6: Sinter the semi-finished material at 1120°C in an inert gas atmosphere (such as helium) for 3.5 hours at a sintering pressure of 50MPa, take it out and air-cool it, then keep it at 960°C for 2.5 hours and then air-cool it, and finally keep it at 335°C for 2 hours to obtain the finished alloy steel-based melt-cast ceramic wear-resistant material.

[0043] Example 2

[0044] Example 2 of the present application discloses a production process of a high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material, comprising the following steps:

[0045] Step 1: Obtain raw materials for preparing a preform, including the following raw materials in percentage by weight:

[0046] Composite ceramic particles 77.5wt%;

[0047] Compound reinforcement particles 20wt%;

[0048] Binder 2.5wt%;

[0049] The particle size of the composite ceramic particles is in the range of 2 to 5 mm, and the composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles in a mass ratio of 2:2:1:1.

[0050] In some embodiments, the particle size of the silicon nitride ceramic particles in the composite ceramic particles is 4-5 mm, the particle size of the zirconium oxide ceramic particles is 2.5-3.5 mm, the particle size of the tungsten carbide ceramic particles is 3-4.5 mm, and the particle size of the yttrium oxide ceramic particles is 2-3 mm.

[0051] In the embodiment of the present application, the particle size of the composite reinforcement particles ranges from 0.5 to 2 mm, and the composite reinforcement particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder, and molybdenum powder in a mass ratio of 6:2:1:1:1;

[0052] Similar to Example 1, the adhesive in this example also uses HR-8767A alumina high temperature adhesive, see Table 1 above for details.

[0053] Step 2: Clean the surfaces of the obtained silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles, yttrium oxide ceramic particles and reinforcement particles, dry them thoroughly and mix them for later use;

[0054] Step 3: Use an electronic weighing tool to correctly mix the binder according to the instructions in Table 1, add the binder to the composite granular material in step 2, first stir and mix at room temperature for 15 minutes; then heat to 190°C at a rate of 120°C / h, stir and mix for 12 minutes; then heat to 350°C at a rate of 100°C / h, stir and mix for 10 minutes; then heat to 530°C at a rate of 80°C / h, stir and mix for 8 minutes; finally heat to 710°C at a rate of 60°C / h, stir and mix for 5 minutes to obtain a premix;

[0055] Step 4: Fill the premix into a mold of a certain shape, and perform warm pressing molding. The heating temperature is 90°C and the pressing pressure is 35MPa. After molding and demolding, let it stand at room temperature for 12 hours, put it in an oven and heat it at 70°C for 3 hours, then heat it to 155°C at a rate of 5°C / min and keep it warm for 2 hours. After slowly cooling, take it out and place it for 24 hours to obtain a ceramic preform.

[0056] Step 5: placing the ceramic preform in the mold, and preheating the ceramic preform and the mold to 870°C, vacuuming after the mold is closed, and then casting the alloy steel molten metal to infiltrate the preform. The casting temperature of the alloy steel molten metal is 1580°C ± 5°C. After the casting is completed, a semi-finished alloy steel-based fused-cast ceramic wear-resistant material is obtained;

[0057] The volume fraction of the ceramic preform in the alloy steel-based fused-cast ceramic wear-resistant material is 30.5vt%. In this embodiment, the alloy steel molten metal contains the following chemical components in percentage by mass:

[0058] Carbon 0.35%, silicon 0.70%, manganese 17.8%, chromium 12.5%, vanadium 1.2%, niobium 0.26%, titanium 0.15%, nitrogen 0.3%, sulfur ≤0.03%, phosphorus ≤0.03%, the balance is Fe and unavoidable impurities, impurity content ≤0.15%.

[0059] Step 6: Sinter the semi-finished material at 1130°C in an inert gas atmosphere for 3.5 hours with a sintering pressure of 50MPa, take it out and air-cool it, then keep it at 970°C for 2.5 hours and then air-cool it, and finally keep it at 345°C for 2 hours to obtain the finished alloy steel-based melt-cast ceramic wear-resistant material.

[0060] Example 3

[0061] Example 3 of the present application discloses a production process of a high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material, comprising the following steps:

[0062] Step 1: Obtain raw materials for preparing a preform, including the following raw materials in percentage by weight:

[0063] Composite ceramic particles 71.5wt%;

[0064] Compound reinforcement particles 25wt%;

[0065] Binder 3.5wt%;

[0066] The particle size of the composite ceramic particles is in the range of 2 to 5 mm, and the composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles in a mass ratio of 2:2:1:1.

[0067] Among them, the particle size of the silicon nitride ceramic particles in the composite ceramic particles is 4-5 mm, the particle size of the zirconium oxide ceramic particles is 2.5-3.5 mm, the particle size of the tungsten carbide ceramic particles is 3-4.5 mm, and the particle size of the yttrium oxide ceramic particles is 2-3 mm.

[0068] In this embodiment, the particle size of the composite reinforcement particles ranges from 0.5 to 2 mm, and the composite reinforcement particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder, and molybdenum powder in a mass ratio of 6:2:1:1:1;

[0069] Similar to Example 1, the adhesive in this example also uses HR-8767A alumina high temperature adhesive, see Table 1 above for details.

[0070] Step 2: Clean the surfaces of the obtained silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles, yttrium oxide ceramic particles and reinforcement particles, dry them thoroughly and mix them for later use;

[0071] Step 3: Use an electronic weighing tool to correctly mix the binder according to the instructions in Table 1, add the binder to the composite granular material in step 2, first stir and mix at room temperature for 15 minutes; then heat to 200°C at a rate of 120°C / h, stir and mix for 12 minutes; then heat to 360°C at a rate of 100°C / h, stir and mix for 10 minutes; then heat to 540°C at a rate of 80°C / h, stir and mix for 8 minutes; finally heat to 720°C at a rate of 60°C / h, stir and mix for 5 minutes to obtain a premix;

[0072] Step 4: Fill the premix into a mold of a certain shape, and perform warm pressing molding. The heating temperature is 100°C, the pressing pressure is 35MPa, and after molding and demolding, it is first allowed to stand at room temperature for 12 hours, and then put into an oven to heat at 80°C for 3 hours, and then heated to 160°C at a rate of 5°C / min for 2 hours. After slowly cooling, take it out and place it for 24 hours to obtain a ceramic preform;

[0073] Step 5: placing the ceramic preform in the mold, and preheating the ceramic preform and the mold to 880°C, vacuuming after the mold is closed, and then casting the alloy steel molten metal to infiltrate the preform. The casting temperature of the alloy steel molten metal is 1580°C ± 5°C. After the casting is completed, a semi-finished alloy steel-based fused-cast ceramic wear-resistant material is obtained;

[0074] The volume fraction of the ceramic preform in the alloy steel-based fused-cast ceramic wear-resistant material is 30.5vt%. In this embodiment, the alloy steel molten metal contains the following chemical components in percentage by mass:

[0075] Carbon 0.35%, silicon 0.70%, manganese 17.8%, chromium 12.5%, vanadium 1.2%, niobium 0.26%, titanium 0.15%, nitrogen 0.3%, sulfur ≤0.03%, phosphorus ≤0.03%, the balance is Fe and unavoidable impurities, impurity content ≤0.15%.

[0076] Step 6: Sinter the semi-finished material at 1140°C in an inert gas atmosphere for 3.5 hours with a sintering pressure of 50MPa, take it out and air-cool it, then keep it at 980°C for 2.5 hours and then air-cool it, and finally keep it at 355°C for 2 to 3 hours to obtain the finished alloy steel-based melt-cast ceramic wear-resistant material.

[0077] Comparative Example 1

[0078] Compared with Example 1, the only difference of this comparative example 1 is:

[0079] The particle size of the composite ceramic particles is 4 mm.

[0080] Comparative Example 2

[0081] Compared with Example 1, the only difference of this Comparative Example 2 is:

[0082] The composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles in a mass ratio of 1:1:1:1.

[0083] Comparative Example 3

[0084] Compared with Example 1, the only difference of this comparative example 3 is:

[0085] The non-compounded reinforced particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder and molybdenum powder in a mass ratio of 1:1:1:1:1.

[0086] Comparative Example 4

[0087] Compared with Example 1, the only difference of this comparative example 4 is:

[0088] The adhesive is replaced by the commonly used epoxy resin adhesive.

[0089] Comparative Example 5

[0090] Compared with Example 1, the only difference of this comparative example 5 is:

[0091] The binder is replaced by the commonly used phenolic resin binder.

[0092] Comparative Example 6

[0093] Compared with Example 1, the only difference of this Comparative Example 6 is:

[0094] Alloy steel is replaced by the commonly used ZGMn13Cr2 high manganese steel.

[0095] Test example

[0096] The alloy steel-based fused-cast ceramic wear-resistant material samples prepared in the above examples and comparative examples were subjected to the following performance tests:

[0097] Table 2: Test data of each group

[0098] Object HV30 <![CDATA[Wear volume / mm 3 > Tensile strength / MPa Yield strength / MPa Example 1 1735 87 856 623 Example 2 1611 94 783 559 Example 3 1508 99 720 504 Comparative Example 1 1420 102 667 441 Comparative Example 2 1531 113 618 405 Comparative Example 3 1609 105 645 422 Comparative Example 4 1247 121 579 367 Comparative Example 5 1176 124 596 380 Comparative Example 6 1653 93 752 538

[0099] Note: The test method for the wear volume in Table 2 is to use an MMH-5 three-body abrasive wear tester, with quartz sand of 40-70 mesh, a test load of 40N, a rotation speed of 50r / min, 20 grinding passes for each sample, and 1h for each grinding pass. The larger the wear volume value, the worse the wear resistance.

[0100] From the records and statistical data in Table 2 above, it can be seen that the hardness, wear resistance and mechanical strength of Example 1 of the present application are better than those of Examples 2-3. Specifically, compared with Examples 2-3, the material of Example 1 is improved by at least 7.70% in hardness, at least 7.45% in wear resistance, at least 9.32% in tensile strength, and at least 11.45% in yield strength. Therefore, the scheme of Example 1 of the present application is the best example, and the schemes of Examples 2 and 3 are suboptimal examples. By setting up comparative experiments, it is found that, based on the best example Example 1, some of the components or contents thereof are changed so that they are not within the scope of protection of the present application, the mechanical properties, hardness and wear resistance of the alloy steel-based fused-cast ceramic wear-resistant material finally prepared all decline to varying degrees. Specifically, compared with Comparative Examples 1-6, the material of Example 1 is improved by 47.53% in hardness, 42.53% in wear resistance, 47.84% in tensile strength, and 69.75% in yield strength.

[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A production process for high-strength integrated alloy steel-based fused-cast ceramic wear-resistant material, characterized in that: The following steps are involved: Step 1: Obtain raw materials for preparing a preform, including the following raw materials in percentage by weight: Composite ceramic particles ≤ 83wt%; Compound reinforcement particles 15-25wt%; Binder 2-3.5wt%; The composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles; the composite reinforcement particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder and molybdenum powder; Step 2: Clean the surfaces of the obtained silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles, yttrium oxide ceramic particles and reinforcement particles, dry them thoroughly and mix them for later use; Step 3: Add the binder to the composite granular material of step 2, first stir and mix at room temperature for 15 minutes; then heat to 180-200°C at a rate of 120°C / h, stir and mix for 12 minutes; then heat to 340-360°C at a rate of 100°C / h, stir and mix for 10 minutes; then heat to 520-540°C at a rate of 80°C / h, stir and mix for 8 minutes; finally heat to 700-720°C at a rate of 60°C / h, stir and mix for 5 minutes to obtain a premix; Step 4: Fill the premix into the mold, warm press molding, the heating temperature is 80-100°C, the pressing pressure is 35MPa, and after molding and demolding, it is first allowed to stand at room temperature for 12 hours, and then put into the oven for heating at 60-80°C for 3 hours, and then heated to 150-160°C at a rate of 5°C / min for 2 hours, and then slowly cooled and taken out for 24 hours to obtain a ceramic preform; Step 5: placing the ceramic preform in a casting mold, and preheating the ceramic preform and the casting mold to 860-880°C, vacuumizing the mold after closing, and then casting the alloy steel molten metal to infiltrate the preform. The casting temperature of the alloy steel molten metal is 1580°C ± 5°C. After the casting is completed, a semi-finished alloy steel-based fused-cast ceramic wear-resistant material is obtained; Step 6: sinter the semi-finished material at 1120-1140° C. in an inert gas atmosphere for 3.5 hours at a sintering pressure of 50 MPa, take it out and air cool it, then keep it at 960-980° C. for 2.5 hours and then air cool it, and finally keep it at 335-355° C. for 2 hours to obtain a finished alloy steel-based melt-cast ceramic wear-resistant material; The particle size of the composite ceramic particles is in the range of 2 to 5 mm; the composite ceramic particles are composed of silicon nitride ceramic particles, zirconium oxide ceramic particles, tungsten carbide ceramic particles and yttrium oxide ceramic particles in a mass ratio of 2:2:1:1; the particle size of the silicon nitride ceramic particles in the composite ceramic particles is 4 to 5 mm, the particle size of the zirconium oxide ceramic particles is 2.5 to 3.5 mm, the particle size of the tungsten carbide ceramic particles is 3 to 4.5 mm, and the particle size of the yttrium oxide ceramic particles is 2 to 3 mm; The particle size of the composite reinforced particles ranges from 0.5 to 2 mm; the composite reinforced particles are composed of carbon black powder, titanium powder, niobium powder, vanadium powder, and molybdenum powder in a mass ratio of 6:2:1:1:1; The adhesive is HR-8767A alumina high temperature adhesive, which is an inorganic ceramic component, can withstand high temperatures of 1730°C, has strong bonding with metals and ceramics, and is resistant to aging and acid and alkali; The alloy steel molten metal contains the following chemical components in mass percentage: carbon 0.35%, silicon 0.70%, manganese 17.8%, chromium 12.5%, vanadium 1.2%, niobium 0.26%, titanium 0.15%, nitrogen 0.3%, sulfur ≤0.03%, phosphorus ≤0.03%, and the remainder is Fe and unavoidable impurities, and the impurity content is ≤0.15%.

2. The production process according to claim 1, characterized in that: The volume fraction of the ceramic preform in the alloy steel-based fused-cast ceramic wear-resistant material is 30.5 vt%.

3. The production process according to claim 1, characterized in that: The raw materials of the preform include the following raw materials in weight percentage: Composite ceramic particles 83wt%; Compound reinforcement particles 15wt%; Binder 2wt%.

Citation Information

Cited By

  • Production method and production device of ceramic composite iron-based wear-resistant casting

    CN122076925A