A wear-resistant steel plate and a method for preparing the same

By rationally designing the chemical composition and process flow of wear-resistant steel plates, and using hot rolling and online quenching processes, the problems of stress corrosion cracking and high costs of wear-resistant steel plates are solved, and the production of high-performance wear-resistant steel plates is realized, reducing production costs and Extend service life.

CN118345316BActive Publication Date: 2024-11-08INNER MONGOLIA UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410783656.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-08
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

The existing wear-resistant steel plates are prone to stress corrosion and cracking during use, resulting in failure, and the production cost of high-performance wear-resistant steel plates is relatively high and the manufacturing cost is relatively high.

Method used

By rationally designing the chemical composition of the steel plate, including appropriate amounts of Cu and rare earth elements, using hot rolling and online direct quenching processes, eliminating offline quenching processes, optimizing smelting and heat treatment steps, controlling carbon and alloy content, and improving the weather resistance and wear resistance of the steel plate. performance.

Benefits of technology

The production of high-hardness, high toughness, wear-resistant steel plates has been achieved, which reduces production costs, improves resistance to atmospheric corrosion, extends service life, and significantly reduces the use of precious metal elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118345316B_ABST
    Figure CN118345316B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of steel materials, and specifically relates to a wear-resistant steel plate and a preparation method thereof. Through reasonable alloy composition design and preparation process optimization, the production of high-hardness and high-toughness wear-resistant steel plates can be achieved through a hot mechanical rolling process and online direct quenching, eliminating the offline quenching process, while improving the atmospheric corrosion resistance of the steel plate, and significantly reducing the use of precious metal elements, thereby reducing the production cost of high-performance wear-resistant steel plates in terms of raw material use and process flow. The wear-resistant steel plate has a tensile strength of ≥1300MPa and an elongation of A 50 ≥15%, surface Vickers hardness 410~580HV, ‑20℃ Charpy U-type longitudinal impact energy ≥45J.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel materials, in particular to a wear-resistant steel plate and a preparation method thereof. Background Art

[0002] Wear-resistant steel plates have high hardness, high wear resistance and excellent strength and toughness, and are widely used in engineering machinery, mining machinery, railway transportation, power equipment, agricultural equipment and other fields. The high strength and hardness of wear-resistant steel plates mainly come from the martensitic matrix structure in the steel. At present, in order to obtain excellent microstructure and improve its wear resistance, the production of high-grade wear-resistant steel plates generally follows a set of refined process flows. This includes the initial hot rolling process, followed by the key heat treatment steps: reheating, quenching and tempering. Each link is precisely controlled to ensure that the steel plate not only has excellent wear resistance, but also maintains good toughness and overall mechanical properties to meet the needs of high-intensity use. Through this consistent process, the microstructure of the wear-resistant steel plate is optimized, ensuring its reliability and service life under harsh working conditions. For example, the Chinese invention patent application with publication number CN111676418A provides a rare earth treated HB500 grade high wear resistant steel plate and its production method, which adopts offline quenching hardening and tempering process after hot rolling to manufacture HB500 grade wear resistant steel plate. This process flow inevitably increases the manufacturing cost.

[0003] Stress corrosion cracking is one of the common failure forms of wear-resistant steel plates during service. Stress corrosion cracking occurs under the combined effects of tensile stress and climatic corrosion environment. It often originates from pitting pits and produces microcracks that are difficult to identify with the naked eye under the action of tensile stress. In the preparation process of wear-resistant steel plates, the tendency of stress corrosion cracking of steel plates is mainly reduced by reducing the carbon content of steel and ensuring that the matrix structure is tempered martensite. Therefore, in order to ensure better stress corrosion resistance, part of the wear resistance of the steel plate is often sacrificed, making the tempering process after quenching a necessary process for wear-resistant steel plates, which significantly increases the manufacturing cost. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a wear-resistant steel plate and a preparation method thereof.

[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0006] A wear-resistant steel plate, which comprises, by weight percentage, C 0.07-0.37%, Si 0.01-0.8%, Mn 0.2-0.65%, Al 0.1-0.65%, Cu 0.5-1.5%, Ni 0.2-1.0%, Cr 0.1-0.9%, Mo 0.01-0.3%, Nb 0-0.005%, Ti 0-0.03%, V 0-0.06%, B 0.001-0.005%, Ca 0.0008-0.003%, RE 0.001-0.0018%, P≤0.012%, S≤0.005%, N≤0.008%, and the remainder is iron and unavoidable impurities.

[0007] As a preferred embodiment of the wear-resistant steel plate described in the present invention, the content ratio of Cu to Ni is ≥1.5, the content ratio of Ti to N is ≥3.5, the content ratio of Ca to S is 1.1-2.0, and the content ratio of Mn to S is 3.4-3.8.

[0008] As a preferred embodiment of the wear-resistant steel plate described in the present invention, the RE is at least one of La and Ce. When RE is La and Ce, the mass ratio of La to Ce is 2:1.

[0009] As a preferred embodiment of the wear-resistant steel plate described in the present invention, the wear-resistant steel plate has a tensile strength of ≥1300 MPa and an elongation of A 50 ≥15%, surface Vickers hardness is 410~580HV, -20℃ Charpy U-type longitudinal impact energy is ≥45J.

[0010] As a preferred embodiment of the wear-resistant steel plate described in the present invention, the microstructure of the wear-resistant steel plate includes: ≥90 vol% martensite, 0-1.5 vol% retained austenite, and the rest is bainite, ferrite or pearlite.

[0011] As a preferred embodiment of the wear-resistant steel plate described in the present invention, the thickness of the wear-resistant steel plate is 7-20 mm.

[0012] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0013] A method for preparing the above-mentioned wear-resistant steel plate comprises the following steps:

[0014] S1, smelting to obtain a casting billet;

[0015] S2, austenitizing the ingot;

[0016] S3, hot rolling the ingot to obtain a hot rolled plate;

[0017] S4, quenching the hot-rolled plate to obtain a quenched plate;

[0018] S5. The quenched plate is tempered and air-cooled to obtain a wear-resistant steel plate.

[0019] As a preferred embodiment of the method for preparing the wear-resistant steel plate described in the present invention, wherein: in the step S1, the smelting process is: molten iron pretreatment - converter steelmaking - LF refining - RH refining - continuous casting; during the RH vacuum treatment, the treatment time is 25-28 minutes, and during the RH vacuum treatment, different contents of Cu-RE alloys are selected according to the components detected at the end of LF refining, and added into the molten steel in the form of wire feeding, and soft blowing is performed after the RH vacuum treatment is completed; sampling is performed in the continuous casting tundish to determine the O and S contents, wherein O≤0.005wt%, S≤0.005wt%, preferably O≤0.002wt%, S≤0.002wt%, and protective casting is adopted throughout the continuous casting process.

[0020] As a preferred embodiment of the method for preparing the wear-resistant steel plate of the present invention, in step S1, during the RH vacuum treatment, different contents of Cu-RE alloy are selected according to the components detected at the end of LF refining, specifically:

[0021] When the O content is less than 0.005wt% and the S content is less than 0.005wt%, Cu-10wt%RE alloy is added to the steel;

[0022] When the O content is 0.005-0.007wt% and the S content is 0.005-0.01wt%, Cu-20wt%RE alloy is added to the molten steel;

[0023] When the O content is greater than 0.007wt% and the S content is greater than 0.01wt%, Cu-30wt%RE alloy is added to the molten steel.

[0024] As a preferred embodiment of the method for preparing the wear-resistant steel plate of the present invention, in the step S2, the ingot is heated to 1200-1300°C and kept at this temperature for 30-150 minutes for austenitization.

[0025] As a preferred embodiment of the method for preparing the wear-resistant steel plate of the present invention, in step S3, the starting rolling temperature is 1080-1150°C, the final rolling temperature is higher than the Ar3 temperature of the steel, the preferred final rolling temperature is 810-960°C, and the more preferred final rolling temperature is 850-950°C. The cumulative reduction rate is 65-75%.

[0026] As a preferred embodiment of the method for preparing the wear-resistant steel plate of the present invention, in step S4, the hot-rolled plate is rapidly cooled to below 480°C, with a cooling rate of not less than 30°C / s, preferably to below 280°C, and more preferably to below 175°C.

[0027] As a preferred embodiment of the method for preparing the wear-resistant steel plate of the present invention, in step S5, the tempering temperature is 100-480° C., and the holding time is 10-50 min.

[0028] The beneficial effects of the present invention are as follows:

[0029] The present invention provides a wear-resistant steel plate and a preparation method thereof. Through reasonable alloy composition design and preparation process optimization, the production of high-hardness and high-toughness wear-resistant steel plates can be achieved through a hot mechanical rolling process and online direct quenching, eliminating the offline quenching process, reducing energy consumption and production costs, and improving the atmospheric corrosion resistance of the steel plate, extending its service life, and significantly reducing the use of precious metal elements. The production cost of high-performance wear-resistant steel plates is reduced in terms of raw material use and process flow. The wear-resistant steel plate has a tensile strength of ≥1300MPa and an elongation of A 50 ≥15%, surface Vickers hardness is 410~580HV, -20℃ Charpy U-type longitudinal impact energy is ≥45J. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0031] Figure 1 This is the metallographic structure diagram of the wear-resistant steel plate prepared in Example 1.

[0032] Figure 2 This is the phase transition point curve of the wear-resistant steel plate prepared in Example 1.

[0033] Figure 3 This is the metallographic structure diagram of the wear-resistant steel plate prepared in Example 2.

[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0035] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The present invention provides a wear-resistant steel plate and a preparation method thereof, which have the following advantages:

[0037] (1) Through reasonable chemical composition design, controlling the carbon and alloy content, and adding appropriate amounts of Cu and rare earth elements to the designed composition, the weather resistance and wear resistance of the steel plate are improved. At the same time, the dendrite segregation of the cast steel plate is reduced, the enrichment of harmful elements at the original austenite grain boundary is hindered, the grains are refined, and the various mechanical properties of the steel plate are effectively improved.

[0038] (2) During RH vacuum treatment, adding Cu-RE alloy to the molten steel by wire feeding can greatly improve the recovery rate of rare earths, ensure the stability of steel performance, and reduce the excessive addition of rare earth elements and Cu elements, thus saving costs.

[0039] (3) The use of hot rolling and direct quenching after rolling eliminates the offline quenching process, shortens the process flow, reduces equipment investment, and saves labor and production costs.

[0040] (4) The precipitation of Cu-rich particles during the tempering process further strengthens the strength of the steel plate without weakening the toughness of the steel plate.

[0041] According to one aspect of the present invention, the present invention provides the following technical solution:

[0042] A wear-resistant steel plate, which comprises, by weight percentage, C 0.07-0.37%, Si 0.01-0.8%, Mn 0.2-0.65%, Al 0.1-0.65%, Cu 0.5-1.5%, Ni 0.2-1.0%, Cr 0.1-0.9%, Mo 0.01-0.3%, Nb 0-0.005%, Ti 0-0.03%, V 0-0.06%, B 0.001-0.005%, Ca 0.0008-0.003%, RE 0.001-0.0018%, P≤0.012%, S≤0.005%, N≤0.008%, and the remainder is iron and unavoidable impurities.

[0043] Preferably, the content ratio of Cu to Ni is ≥1.5, the content ratio of Ti to N is ≥3.5, the content ratio of Ca to S is 1.1-2.0, and the content ratio of Mn to S is 3.4-3.8; the RE is at least one of La and Ce, and when RE is La and Ce, the mass ratio of La to Ce is 2:1.

[0044] The chemical composition of the wear-resistant steel plate of the present invention is:

[0045] Carbon (C): Carbon can improve the strength and hardness of steel through solid solution strengthening. If the carbon content is less than 0.15wt%, the hardness of the wear-resistant steel plate is difficult to reach 420HV or above, but too much carbon will have an adverse effect on the weldability, toughness, formability and stress corrosion resistance of the steel. Therefore, the present invention sets the carbon content in the range of 0.07~0.37wt%, preferably in the range of 0.15~0.30wt%.

[0046] Silicon (Si): As a deoxidizer in molten steel, silicon can effectively remove oxygen from the molten steel, and can dissolve into the iron matrix lattice after solidification, achieving the effect of solid solution strengthening. At the same time, silicon can promote the formation of an oxide layer and improve the corrosion resistance of steel. However, a silicon content higher than 0.5wt% will reduce the welding performance of the steel plate. Therefore, the present invention sets the silicon content in the range of 0.01~0.8wt%, with a preferred range of 0.04~0.58wt%.

[0047] Manganese (Mn): Manganese can expand the austenite zone, improve the hardenability of steel, reduce the martensitic transformation start (Ms) and end temperature (Mf), and improve the matrix strength through solid solution strengthening. However, manganese will also inhibit the self-tempering of martensite during quenching. Although a lower degree of martensite self-tempering will increase the matrix hardness, it also increases the risk of quenching cracking and deformation, and has an adverse effect on impact toughness. At the same time, excessive manganese will also lead to C-Mn segregation and the formation of MnS, resulting in pitting and stress corrosion cracking. Therefore, the present invention sets the manganese content to 0.2~0.65wt%, preferably in the range of 0.42~0.58wt%, and the Mn to S content ratio is 3.4~3.8.

[0048] Aluminum (Al): Aluminum can not only act as a deoxidizer, but also form AlN with nitrogen (N) to refine the grain structure. However, excessive aluminum will increase the non-metallic inclusions in the steel and reduce the cleanliness of the steel. Therefore, the present invention sets the aluminum content to Al0.1~0.65wt%, preferably in the range of 0.15~0.5wt%.

[0049] Copper (Cu): Copper can promote the formation of an oxide protective layer on steel, improve the atmospheric corrosion resistance of wear-resistant steel plates, and inhibit the occurrence of stress corrosion cracks. At the same time, supersaturated copper will precipitate in the form of regular particles during the tempering process, which will strengthen the steel plate. However, excessive copper will cause copper brittleness during thermal deformation of steel and will also reduce the toughness of the heat-affected zone of welding. Therefore, the present invention sets the copper content to 0.5~1.5wt%, with a preferred range of 0.7~1.1wt%.

[0050] Nickel (Ni): Nickel can improve the hardenability of austenite and increase the strength of steel without losing toughness. Nickel can also improve the steel plate's resistance to pitting corrosion, promote the formation of an oxidation protective layer, improve atmospheric corrosion resistance, and inhibit the stress corrosion behavior of wear-resistant steel plates. However, excessive nickel will promote the production of high-viscosity iron oxide scales, thereby reducing the surface quality of the steel; at the same time, a higher nickel content will also increase the carbon equivalent and crack sensitivity coefficient and have a negative impact on welding performance. In addition, nickel is a precious metal element, and excessive content will significantly increase the cost of the steel plate. Therefore, the present invention sets the nickel content to 0.2~1.0wt%, with a preferred range of 0.25~0.85wt%.

[0051] In order to increase the nucleation rate of the second phase particles rich in Cu during the tempering process, Ni and Al elements should be added. Density functional theory calculations show that in the bcc-Fe matrix, the binding energies of Ni and Al atoms with Cu atoms at the first nearest neighbor are -0.149eV and -0.187eV, respectively, showing an obvious attraction. Therefore, the Ni and Al elements dissolved in the matrix can promote the formation of Cu-rich clusters by Cu atoms during the tempering process. During the growth of the Cu-rich clusters, the Ni and Al atoms in the core of the particles continue to diffuse to the outside of the particles, and finally form a NiAl shell with a B2 crystal structure between the Cu particles and the matrix. The lattice mismatch between this B2-NiAl and the matrix bcc-Fe is extremely low, which effectively reduces the interface energy between the Cu-rich particles and the matrix, thereby improving the thermal stability of the Cu-rich particles and reducing their growth and coarsening tendency, so that nano-scale Cu-rich particles are precipitated and dispersed in the matrix during the tempering process of the steel plate. The experimental results show that in order to achieve the above-mentioned effects of Ni and Al on the nucleation rate and thermal stability of Cu-rich particles, the content ratio of Cu to Ni should be ≥1.5, and the content of Al should be between 0.15 and 0.5wt%.

[0052] Chromium (Cr): Chromium can increase the hardenability of austenite and improve the strength and hardness of steel. Nickel can promote the formation of a dense oxide protective layer in steel, improve the atmospheric corrosion resistance; at the same time, it improves the electrochemical corrosion resistance of steel, thereby preventing stress corrosion. However, excessive chromium will reduce the toughness of the heat-affected zone of welding. Therefore, the present invention sets the chromium content to 0.1~0.9wt%, preferably in the range of 0.25~0.8wt%.

[0053] Molybdenum (Mo): Molybdenum can refine grains, improve strength and toughness, and reduce the temper brittleness of steel. In boron (B) steel, the addition of molybdenum can ensure the expected effect of boron in the steel. At the same time, the molybdenum element can also delay the recrystallization behavior through dragging during the hot deformation of the steel, thereby increasing the aspect ratio of the original austenite grains and ensuring the impact toughness of the finished steel plate. However, it should also be considered that excessive molybdenum will cause excessive elongation of the original austenite grains, thereby reducing the bending performance of the steel plate. In addition, molybdenum is a precious metal element, and too high a content will significantly increase the cost of the steel plate. Therefore, the present invention sets the molybdenum content to 0.01~0.3%, with a preferred range of 0.06~0.28%.

[0054] Niobium (Nb): Niobium can form carbide or carbonitride precipitation phases, refine grains through solid solution drag and precipitation phase pinning, thereby improving the strength and toughness of steel. However, too high a niobium content will reduce the bending properties of steel after direct quenching. Therefore, the present invention sets the niobium content to 0-0.005wt%.

[0055] Titanium (Ti): Titanium can form TiC precipitated particles with carbon. TiC can not only achieve a strengthening effect, but also capture a large amount of hydrogen, reduce the diffusion of hydrogen in steel, and prevent stress corrosion cracking. Titanium can also form TiN with nitrogen (N), preventing excessive growth of austenite grains in the ingot during the high-temperature heating stage before rolling. TiN particles can also prevent grain coarsening in the heat-affected zone of welding, thereby improving the toughness of the heat-affected zone. At the same time, the formation of TiN can reduce the precipitation of BN, so that boron (B) can more fully play its role in enhancing hardenability. However, excessive titanium will cause TiN coarsening and excessive formation of TiC in the steel, thereby reducing the toughness of the steel plate. Therefore, the present invention sets the titanium content at 0~0.03wt%. If the nitrogen content in the steel is less than 0.003wt%, titanium may not be added.

[0056] Vanadium (V): The function of vanadium is the same as that of niobium. The content of vanadium is set at 0-0.06wt% in the present invention.

[0057] Boron (B): Boron can improve the hardenability of steel. However, since boron and nitrogen are easy to form BN, titanium should be added together with boron under nitrogen-containing conditions to preferentially form TiN, thereby avoiding the formation of BN and ensuring the alloying effect of single substance B. The present invention sets the boron content at 0.001-0.005wt%.

[0058] Calcium (Ca): Calcium has the effects of desulfurization and deoxidation, and improves the morphology of non-metallic inclusions and the mechanical properties of steel. The present invention sets the content of calcium to 0.0008-0.003wt%. To avoid the formation of CaS, the content ratio of Ca to S should be in the range of 1.1-2.0.

[0059] Rare earth (La and Ce): Rare earth can purify molten steel, improve cast dendrite segregation, and hinder the segregation of harmful elements at the grain boundary, thereby purifying the grain boundary. Rare earth helps to refine the grains of steel and improve the mechanical properties of steel. Rare earth elements can also improve the distribution and morphology of carbides in steel, thereby promoting precipitation strengthening of steel and effectively strengthening the steel matrix. The present invention sets the content of rare earth at 0.001~0.0018wt%.

[0060] Preferably, the tensile strength of the wear-resistant steel plate is ≥1300MPa, and the elongation A 50 ≥15%, surface Vickers hardness is 410~580HV, -20℃ Charpy U-type longitudinal impact energy is ≥45J.

[0061] Preferably, the microstructure of the wear-resistant steel plate includes: ≥90 vol% martensite, 0-1.5 vol% retained austenite, and the rest is bainite, ferrite or pearlite.

[0062] Preferably, the thickness of the wear-resistant steel plate is 7-20 mm; the original austenite grain size measured in the 1 / 4 thickness area of ​​the plate is ≤50 μm, preferably ≤25 μm; the aspect ratio of the original austenite grain is 1.5-3.5, preferably 2.0-3.0.

[0063] According to another aspect of the present invention, the present invention provides the following technical solution:

[0064] A method for preparing the above-mentioned wear-resistant steel plate comprises the following steps:

[0065] S1, smelting to obtain a casting billet;

[0066] S2, austenitizing the ingot;

[0067] S3, hot rolling the ingot to obtain a hot rolled plate;

[0068] S4, quenching the hot-rolled plate to obtain a quenched plate;

[0069] S5. The quenched plate is tempered and air-cooled to obtain a wear-resistant steel plate.

[0070] Preferably, in step S1, the smelting process is: molten iron pretreatment - converter steelmaking - LF refining - RH refining - continuous casting; during RH vacuum treatment, the treatment time is 25-28 min, during RH vacuum treatment, different contents of Cu-RE alloy are selected according to the components detected at the end of LF refining, and added into the molten steel in the form of wire feeding, and soft blowing is performed after the RH vacuum treatment is completed; sampling is performed in the continuous casting tundish to determine the O and S contents, wherein O≤0.005wt%, S≤0.005wt%, preferably O≤0.002wt%, S≤0.002wt%, and protective casting is adopted throughout the continuous casting process.

[0071] Preferably, in step S1, during the RH vacuum treatment, different contents of Cu-RE alloy are selected according to the components detected at the end of LF refining, specifically:

[0072] When the O content is less than 0.005wt% and the S content is less than 0.005wt%, an alloy of Cu-10wt%RE is added to the steel;

[0073] When the O content is 0.005-0.007wt% and the S content is 0.005-0.01wt%, a Cu-20wt%RE alloy is added to the molten steel;

[0074] When the O content is greater than 0.007wt% and the S content is greater than 0.01wt%, a Cu-30wt%RE alloy is added to the molten steel.

[0075] Preferably, in step S2, the ingot is heated to 1200-1300° C. and kept warm for 30-150 min for austenitization.

[0076] Preferably, in step S3, the starting rolling temperature is 1080-1150° C., the final rolling temperature is higher than the Ar3 temperature of the steel, the preferred final rolling temperature is 810-960° C., and the more preferred final rolling temperature is 850-950° C. The cumulative reduction ratio is 65-75%.

[0077] Preferably, in step S4, the hot-rolled plate is rapidly cooled to below 480°C, with a cooling rate of not less than 30°C / s, preferably to below 280°C, and more preferably to below 175°C.

[0078] Preferably, in step S5, the tempering temperature is 100-480° C., and the holding time is 10-50 min.

[0079] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0080] The performance test method of each embodiment and comparative example is as follows: According to GB / T13239-2006, a FL4000SZ universal tensile machine is used to stretch at a constant chuck moving rate of 1mm / min, and its tensile properties are tested, and the test results are the average of 3 samples. According to GB / T229-2007 standard, a JB-300s digital drop hammer impact test machine is used to test the impact toughness at -20°C, and the experimental results are the average of 3 samples. A Q10A+ fully automatic Vickers hardness tester is used for hardness testing, and the experimental results are the average of 8 points.

[0081] Example 1

[0082] A wear-resistant steel plate comprises, by weight percentage, 0.156% C, 0.225% Si, 0.532% Mn, 0.112% Al, 0.56% Cu, 0.287% Ni, 0.649% Cr, 0.03% Mo, 0.001% Nb, 0.001% B, 0.001% Ca, 0.0015% RE, 0.009% P, 0.002% S, and the remainder is iron and unavoidable impurities.

[0083] The above-mentioned method for preparing the wear-resistant steel plate comprises the following steps:

[0084] S1. Smelting to obtain ingot; the smelting process is: molten iron pretreatment - converter steelmaking - LF refining - RH refining - continuous casting; during RH vacuum treatment, the treatment time is 25min, during RH vacuum treatment, according to the composition detected at the end of LF refining (O content is 0.006wt%, S content is 0.007wt%), Cu-20wt%RE is selected and added into the molten steel in the form of wire feeding, and soft blowing is performed after the RH vacuum treatment is completed; sampling is performed in the continuous casting tundish to determine the O and S contents, wherein O is 0.002wt% and S is 0.002wt%, and protective casting is adopted throughout the continuous casting process;

[0085] S2, heating the ingot to 1250°C and keeping the temperature for 120 minutes for austenitizing;

[0086] S3, hot rolling the ingot to obtain hot rolled plate; the starting rolling temperature is 1090°C, the final rolling temperature is 920°C, and the cumulative reduction rate is 69.5%;

[0087] S4, quenching the hot-rolled plate to obtain a quenched plate; rapidly cooling the hot-rolled plate to 175° C. at a cooling rate of 35° C. / s;

[0088] S5. The quenched plate is tempered at 180°C for 15 minutes, and then air-cooled on a cooling bed to obtain a wear-resistant steel plate.

[0089] The metallographic structure of the wear-resistant steel plate prepared in this embodiment is as follows: Figure 1 As shown by Figure 1 It can be seen that the microstructure of the steel plate is mainly martensite; the phase transition point of the steel plate after austenitization in step S2 is detected, and the sample is heated to 1150℃ at a heating rate of 0.05℃ / s using L78RITA quenching thermal expansion instrument. The critical phase transition points Ac1 and Ac3 of the wear-resistant steel plate are obtained during the heating process. The Ms of the wear-resistant steel is obtained during the cooling process of the sample to room temperature at a cooling rate of 180℃ / s. The results are as follows Figure 2, Ac1=743.0℃, Ac3=865.4℃, Ms=398.6℃. The wear-resistant steel plate prepared in this embodiment was tested for performance, and its tensile strength was 1317MPa, ductility A 50 The surface Vickers hardness is 417HV, and the -20℃ Charpy U-type longitudinal impact energy is 51J.

[0090] Example 2

[0091] The difference from Example 1 is that the wear-resistant steel plate, by weight percentage, has the following composition: C 0.159%, Si 0.314%, Mn 0.584%, Al 0.145%, Cu 0.76%, Ni 0.304%, Cr 0.647%, Mo 0.04%, Nb 0.001%, B 0.0025%, Ca 0.0015%, RE 0.0016%, P 0.009%, S 0.002%, and the rest is iron and inevitable impurities; in step S3, the ingot is hot rolled to obtain a hot-rolled plate; the starting rolling temperature is 1130° C., and the finishing rolling temperature is 925° C.; in step S4, the hot-rolled plate is rapidly cooled to 175° C., and the cooling rate is 37° C. / s.

[0092] The metallographic structure of the wear-resistant steel plate prepared in this embodiment is as follows: Figure 3 As shown by Figure 3 It can be seen that the microstructure of the steel plate is mainly martensite; the wear-resistant steel plate prepared in this embodiment is tested for performance, and its tensile strength is 1523MPa, elongation A 50 The surface Vickers hardness is 462HV, and the -20℃ Charpy U-type longitudinal impact energy is 63J.

[0093] Example 3

[0094] The difference from Example 2 is that the wear-resistant steel plate, by weight percentage, has the following composition: C 0.164%, Si 0.432%, Mn 0.645%, Al 0.236%, Cu 1.06%, Ni 0.341%, Cr 0.648%, Mo 0.05%, Nb 0.002%, B 0.004%, Ca 0.002%, RE 0.0012%, P 0.007%, S 0.002%, and the rest are iron and unavoidable impurities; the final rolling temperature in step S3 is 927°C.

[0095] The wear-resistant steel plate prepared in this embodiment was tested for its performance, and its tensile strength was 1723MPa and its elongation was A 50 The surface Vickers hardness is 554HV, and the -20℃ Charpy U-type longitudinal impact energy is 70J.

[0096] Example 4

[0097] The difference from Example 2 is that the wear-resistant steel plate has the following composition, by weight percentage: C 0.186%, Si 0.465%, Mn 0.623%, Al 0.358%, Cu 1.21%, Ni 0.264%, Cr 0.732%, Mo 0.07%, Nb 0.003%, B 0.002%, V 0.005%, Ca 0.001%, RE 0.0015%, P 0.008%, S 0.003%, and the rest is iron and unavoidable impurities.

[0098] The wear-resistant steel plate prepared in this embodiment was tested for its performance, and its tensile strength was 1763MPa and its elongation was A 50 The surface Vickers hardness is 571HV, and the -20℃ Charpy U-type longitudinal impact energy is 72J.

[0099] Comparative Example 1

[0100] The difference from Example 1 is that the wear-resistant steel plate has the following composition, by weight percentage: C 0.151%, Si 0.378%, Mn 1.406%, Al 0.017%, Ni 0.018%, Cr 0.911%, Mo 0.276%, Nb 0.028%, P 0.013%, S 0.005%, and the rest is iron and unavoidable impurities.

[0101] The wear-resistant steel plate prepared in this comparative example was tested for performance, and its tensile strength was 1216MPa, elongation A 50 The surface Vickers hardness is 396HV, and the -20℃ Charpy U-type longitudinal impact energy is 43J.

[0102] Comparative Example 2

[0103] The difference from Example 1 is that during the RH vacuum treatment in S1, Fe-20%RE and Fe-20%Cu alloys in the same content as in Example 1 are added to the molten steel by wire feeding. The wear-resistant steel plate has the following components by weight percentage: C 0.148%, Si 0.368%, Mn 1.406%, Al 0.026%, Cu 0.36%, Ni 0.015%, Cr 0.921%, Mo 0.256%, Nb 0.027%, B 0.001%, Ca 0.001%, RE 0.0003%, P 0.015%, S 0.005%,

[0104] The wear-resistant steel plate prepared in this comparative example was tested for performance, and its tensile strength was 1234 MPa and its elongation was A 50The surface Vickers hardness is 401HV, and the -20℃ Charpy U-type longitudinal impact energy is 45J.

[0105] Comparative Example 3

[0106] The difference from Example 1 is that the final rolling temperature in step S3 is 750°C.

[0107] The wear-resistant steel plate prepared in this comparative example was tested for performance, and its tensile strength was 1073MPa and its elongation was A 50 The surface Vickers hardness is 312HV, and the -20℃ Charpy U-type longitudinal impact energy is 37J.

[0108] It can be seen from the embodiments of the present invention and the comparative examples that the present invention can realize the production of high-hardness, high-toughness wear-resistant steel plates through reasonable alloy composition design and preparation process optimization, through hot mechanical rolling process and online direct quenching, eliminating the offline quenching process, while improving the atmospheric corrosion resistance of the steel plate, and significantly reducing the use of precious metal elements, reducing the production cost of high-performance wear-resistant steel plates in terms of raw material use and process flow, and the tensile strength of the wear-resistant steel plate is ≥1300MPa, and the elongation A is ≥1300MPa. 50 ≥15%, surface Vickers hardness is 410~580HV, -20℃ Charpy U-type longitudinal impact energy is ≥45J.

[0109] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a wear-resistant steel plate, characterized in that: The steps include: S1. Smelting to obtain ingots; the smelting process is: molten iron pretreatment - converter steelmaking - LF refining - RH refining - continuous casting; during RH refining, different contents of Cu-RE alloys are selected according to the components detected at the end of LF refining, specifically: When the O content is less than 0.005wt% and the S content is less than 0.005wt%, Cu-10wt%RE alloy is added to the molten steel; When the O content is 0.005-0.007wt% and the S content is 0.005-0.01wt%, Cu-20wt%RE alloy is added to the molten steel; When the O content is greater than 0.007wt% and the S content is greater than 0.01wt%, Cu-30wt%RE alloy is added to the molten steel; S2, austenitizing the ingot; heating the ingot to 1250-1300°C and keeping the temperature for 30-150 minutes for austenitizing; S3, hot rolling of the ingot to obtain hot rolled plate; the starting rolling temperature is 1080~1150℃, the final rolling temperature is higher than the Ar3 temperature of the steel, and the cumulative reduction rate is 65~75%; S4, quenching the hot-rolled plate to obtain a quenched plate; S5, the quenched plate is tempered at a temperature of 100-180°C for a holding time of 10-15 minutes, and then air-cooled to obtain a wear-resistant steel plate; The wear-resistant steel plate is composed of C 0.07-0.186%, Si 0.01-0.8%, Mn 0.2-0.58%, Al 0.15-0.5%, Cu 0.5-1.5%, Ni 0.2-1.0%, Cr 0.1-0.732%, Mo 0.01-0.3%, Nb 0-0.001%, V0-0.06%, B 0.001-0.005%, Ca 0.0008-0.003%, RE 0.001-0.0018%, P≤0.012%, S≤0.005%, N≤0.008%, and the rest are iron and unavoidable impurities; the content ratio of Cu to Ni is ≥1.5; the tensile strength of the wear-resistant steel plate is ≥1523MPa, the elongation A 50 ≥15%, surface Vickers hardness 410~580HV, -20℃ Charpy U-type longitudinal impact energy ≥45J; The microstructure of the wear-resistant steel plate includes: ≥90 vol% of martensite, 0-1.5 vol% of retained austenite, and the rest is bainite, ferrite or pearlite.

2. The method for preparing the wear-resistant steel plate according to claim 1, characterized in that: The RE is at least one of La and Ce. When RE is La and Ce, the mass ratio of La to Ce is 2:

1.

3. The method for preparing the wear-resistant steel plate according to claim 1, characterized in that: In the step S4, the hot-rolled plate is rapidly cooled to below 480°C, with a cooling rate of not less than 30°C / s.