A kind of weather-resistant adhesive and preparation method thereof

Through the catalytic reaction of modified bio-based and nickel salts, combined with styrene-acrylic emulsion, aluminum sulfate and gelatin, a weather-resistant adhesive is prepared, which solves the problem of insufficient durability of traditional adhesives in high temperature and high humidity environments, and achieves high bonding strength and Environmentally friendly adhesive preparation broadens the application scope of biomass-based adhesives.

CN118374264BActive Publication Date: 2024-10-15GUANGDONG YAQIAO NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410614938.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-16
Publication Date
2024-10-15
Estimated Expiration
2044-05-16

AI Technical Summary

Technical Problem

Traditional epoxy adhesives have insufficient durability in high-temperature and high-humidity environments. Existing biomass-based adhesives have limited application range and are difficult to meet diverse performance needs.

Method used

A combination of modified bio-based, styrene-acrylic emulsion, aluminum sulfate and gelatin is used to modify the lignin through a nickel salt catalytic reaction to improve the viscosity and bonding effect. The weather-resistant adhesive is prepared by heating the reaction in a nitrogen atmosphere.

Benefits of technology

The prepared adhesive has high weather resistance and bonding strength, reduces the use of organic solvents and harmful substances, is suitable for indoor and outdoor environments, maintains stable bonding strength, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a weather-resistant adhesive and a preparation method thereof. The raw materials include 50-70 parts of modified bio-based materials, 20-25 parts of styrene-acrylic emulsions, 0.5-1 parts of aluminum sulfate and 5-9 parts of gelatin by weight. The preparation method of the high weather-resistant adhesive is to mix water, styrene-acrylic emulsion and modified bio-based materials to obtain a reaction material 1, adjust the pH of the mixed material 1 to 3-5, add aluminum sulfate and gelatin, stir at 200-300r / min for 50-70min at 80-90°C, and obtain a high weather-resistant adhesive. The high weather-resistant adhesive obtained by the invention is green and environmentally friendly, and has a good bonding effect under high temperature and high humidity environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesive preparation, and in particular to a method for preparing a weather-resistant adhesive. Background Art

[0002] The weather resistance of an adhesive refers to the durability of the adhesive under natural environmental conditions, such as temperature, humidity, light, oxygen, ozone, water, and various chemical media.

[0003] Epoxy resin is a widely used adhesive material, but traditional epoxy adhesives often fail to meet today's diverse performance requirements and need to be modified with chemical reagents before use. In order to protect the environment and achieve sustainable development of adhesives, the synthesis of bio-based epoxy adhesives, the improvement of biocomponent content and material performance have gradually become one of the research and development hotspots of epoxy resin adhesives. Prior art CN114369435A is a method for preparing a biomass-based adhesive and an adhesive, wherein a biomass raw material is hydrolyzed and filtered in an acidic solution to obtain a biomass hydrolyzate rich in aldehydes; a biomass raw material rich in lignin and a lignin activation additive are added to an alkaline solution for activation to obtain activated lignin; the biomass hydrolyzate and activated lignin react in an alkaline solution to obtain a biomass-based adhesive. The biomass-based adhesive prepared by this preparation method is mainly used in the bonding of household panels, and the use effect of the biomass-based adhesive in a high temperature and high humidity environment is not recorded. In order to broaden the scope of application of biomass-based adhesives, the present invention proposes a method for preparing a weather-resistant adhesive Summary of the invention

[0004] In view of this, the present invention proposes a method for preparing a high-weatherability adhesive to solve the above problems.

[0005] The technical solution of the present invention is achieved in this way:

[0006] A weather-resistant adhesive comprises raw materials, by weight, including 50-70 parts of modified bio-based materials, 20-25 parts of styrene-acrylic emulsion, 0.5-1 parts of aluminum sulfate and 5-9 parts of gelatin.

[0007] Furthermore, the modified bio-based material is prepared by mixing lignin, a metal catalyst and water, and heating the mixture under a nitrogen atmosphere for reaction.

[0008] Furthermore, the metal catalyst is a nickel salt.

[0009] Furthermore, the nickel salt is one of nickel nitrate, nickel sulfate and nickel chloride.

[0010] Furthermore, the nickel salt is nickel nitrate.

[0011] Furthermore, the mass ratio of the lignin, the metal catalyst and water is 1:0.1-0.2:100-150.

[0012] Furthermore, the reaction is carried out at 500-600° C. for 6-8 hours under a nitrogen atmosphere.

[0013] Furthermore, the nitrogen pressure is 0.3-0.7Mpa.

[0014] Furthermore, the mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion is 0.8-1:1.

[0015] Further, the preparation method of the weather-resistant adhesive comprises the following steps:

[0016] (1) mixing water, styrene acrylic emulsion and modified bio-based material to prepare a mixed material 1;

[0017] (2) The pH of the mixed material 1 is adjusted to 3-5, and aluminum sulfate and gelatin are added and mixed to prepare a weather-resistant adhesive.

[0018] Furthermore, in step (1), the amount of water used is 30-40% of the total mass of the styrene-acrylic emulsion and the modified bio-based material.

[0019] Furthermore, in step (2), the mixing is performed by stirring at 200-300 r / min for 50-70 min at 80-90°C.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The weather-resistant adhesive of the present invention is prepared by using modified bio-based materials, styrene-acrylic emulsion, aluminum sulfate and gelatin. The prepared adhesive has high weather resistance and bonding strength. The addition of organic solvents and harmful substances in the raw materials of the present invention is reduced. The prepared adhesive is environmentally friendly and meets environmental protection requirements.

[0022] The modified bio-based material in the present invention uses lignin as a raw material and uses a catalyst containing a nickel salt to react. The functional groups such as phenolic hydroxyl groups and aliphatic hydroxyl groups in the modified lignin interact with other lignin molecules or solvent molecules through hydrogen bonds, thereby increasing the viscosity of the modified bio-based material and improving the fluidity of lignin in the solvent, which is beneficial to improving the bonding effect of the adhesive. The nickel salt of the present invention can also participate in the preparation of the adhesive to improve the curing effect of the adhesive.

[0023] The invention adds styrene acrylic emulsion, aluminum sulfate and gelatin, which can improve the water resistance and high temperature resistance of the adhesive, prevent it from becoming soft or falling off due to moisture, maintain stable bonding strength, and is suitable for indoor and outdoor environments. DETAILED DESCRIPTION

[0024] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0025] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0026] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0027] The lignin used in the present invention is straw lignin.

[0028] Example 1

[0029] (1) Lignin, nickel nitrate and water were mixed in a mass ratio of 1:0.1:100, and the temperature was increased to 500°C at 5°C / min in a nitrogen atmosphere of 0.3 MPa for 6 h to obtain a modified bio-based material.

[0030] (2) By weight, 50 parts of modified bio-based materials, 20 parts of styrene-acrylic emulsion, 0.5 parts of aluminum sulfate, and 5 parts of gelatin were weighed, wherein the mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion was 0.9:1.

[0031] (3) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water used is 30% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1;

[0032] (4) The pH of the mixed material 1 was adjusted to 3 with a 2 mol / L phosphoric acid solution, and aluminum sulfate and gelatin were added. The mixture was stirred at 200 r / min at 80° C. for 50 min to prepare a weather-resistant adhesive.

[0033] Example 2

[0034] (1) Lignin, nickel nitrate and water were mixed in a mass ratio of 1:0.15:130, and the temperature was increased to 550°C at 5°C / min for 7 hours in a nitrogen atmosphere of 0.5 MPa to obtain a modified bio-based material.

[0035] (2) By weight, 60 parts of modified bio-based materials, 23 parts of styrene-acrylic emulsion, 0.8 parts of aluminum sulfate, and 7 parts of gelatin were weighed, wherein the mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion was 0.9:1.

[0036] (3) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water is 35% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1;

[0037] (4) The pH of the mixed material 1 was adjusted to 4 with a 2 mol / L phosphoric acid solution, and aluminum sulfate and gelatin were added thereto. The mixture was stirred at 250 r / min for 60 min at 85° C. to prepare a weather-resistant adhesive.

[0038] Example 3

[0039] (1) Lignin, nickel nitrate and water were mixed in a mass ratio of 1:0.2:150, and the temperature was increased to 600°C at 5°C / min in a nitrogen atmosphere of 0.7 MPa for 8 h to obtain a modified bio-based material.

[0040] (2) According to weight, 70 parts of modified bio-based materials, 25 parts of styrene-acrylic emulsion, 1 part of aluminum sulfate, and 9 parts of gelatin were weighed, wherein the mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion was 0.9:1.

[0041] (3) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water is 40% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1;

[0042] (4) The pH of the mixed material 1 was adjusted to 5 with a 2 mol / L phosphoric acid solution, and aluminum sulfate and gelatin were added thereto. The mixture was stirred at 300 r / min for 70 min at 90° C. to prepare a weather-resistant adhesive.

[0043] Test Example 1

[0044] The adhesive prepared in Examples 1-3 was tested according to the national standard GB / T17657-2013 "Test Methods for Physical and Chemical Properties of Artificial Boards and Facing Artificial Boards". The specimens were made of poplar wood with a specification of 25mm×100mm, a thickness of 2mm, and a moisture content of less than 15%. The adhesive coating amount was 250g / ㎡. After the specimens were coated with the adhesive, they were pressed at 200℃ and 1MPa for 5min. After cooling, they were immersed in 63℃ hot water and 93℃ hot water for 3h respectively. Each specimen was stretched and broken at a speed of 2mm / min within 30s. Each experimental group was repeated 3 times and the average value was taken.

[0045] name Example 1 Example 2 Example 3 Untreated shear strength (MPa) 3.84 4.05 3.96 Re-dry strength after immersion in hot water at 63℃ for 3h (MPa) 3.71 3.97 3.89 Re-dry strength after immersion in 93℃ hot water for 3h (MPa) 3.55 3.91 3.78

[0046] The experimental results show that the adhesive prepared by the present invention has a very good bonding effect and good weather resistance, and the bonding effect does not show a significant decrease under high temperature conditions.

[0047] Comparative Example 1

[0048] Based on Example 2, the raw material components were adjusted, specifically:

[0049] (1) Lignin, nickel nitrate and water were mixed in a mass ratio of 1:0.15:130, and the temperature was increased to 550°C at 5°C / min for 7 hours in a nitrogen atmosphere of 0.5 MPa to obtain a modified bio-based material.

[0050] (2) By weight, weigh 60 parts of modified bio-based materials, 23 parts of styrene-acrylic emulsion, and 0.8 parts of aluminum sulfate. The mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion is 0.9:1.

[0051] (3) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water is 35% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1;

[0052] (4) The mixture 1 was adjusted to pH 4 with a 2 mol / L phosphoric acid solution, aluminum sulfate was added, and the mixture was stirred at 85° C. and 250 r / min for 60 min to prepare a weather-resistant adhesive.

[0053] The untreated shear strength of the adhesive prepared in Comparative Example 1 is 3.15MPa, the re-dry strength after soaking in hot water at 63°C for 3h is 2.84MPa, and the re-dry strength after soaking in hot water at 93°C for 3h is 2.37MPa. The test results show that the addition of gelatin can improve the bonding effect of the adhesive, and the bonding effect is significantly reduced in boiling water at 93°C. Gelatin not only has a good bonding effect on the substrate, but also gelatin can further improve the mixing effect of the modified bio-based and styrene-acrylic emulsion to form a uniform mixture; at the same time, the active sites in the gelatin and the modified bio-based react to improve the stability of the gelatin, further improving the overall bonding effect of the adhesive.

[0054] Comparative Example 2

[0055] The raw material ratio was adjusted based on Example 2, specifically,

[0056] (1) Lignin, nickel nitrate and water were mixed in a mass ratio of 1:0.15:130, and the temperature was increased to 550°C at 5°C / min for 7 hours in a nitrogen atmosphere of 0.5 MPa to obtain a modified bio-based material.

[0057] (2) According to weight, 70 parts of modified bio-based materials, 40 parts of styrene-acrylic emulsion, 1 part of aluminum sulfate, and 9 parts of gelatin were weighed, wherein the mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion was 0.9:1.

[0058] (3) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water is 35% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1;

[0059] (4) The pH of the mixed material 1 was adjusted to 4 with a 2 mol / L phosphoric acid solution, and aluminum sulfate and gelatin were added thereto. The mixture was stirred at 250 r / min for 60 min at 85° C. to prepare a weather-resistant adhesive.

[0060] The untreated shear strength of the adhesive prepared in Comparative Example 2 is 3.32 MPa, the re-dry strength after immersion in hot water at 63°C for 3 hours is 3.17 MPa, and the re-dry strength after immersion in hot water at 93°C for 3 hours is 2.89 MPa. The test results show that the ratio of raw materials affects the bonding properties of the adhesive.

[0061] Comparative Example 3

[0062] The preparation method of the modified bio-based material was adjusted based on Example 2, specifically:

[0063] (1) Lignin, nickel nitrate and water were mixed in a mass ratio of 1:0.15:130, and the mixture was heated to 700°C at 10°C / min in a nitrogen atmosphere of 0.5 MPa for 5 h to obtain a modified bio-based material.

[0064] (2) By weight, 60 parts of modified bio-based materials, 23 parts of styrene-acrylic emulsion, 0.8 parts of aluminum sulfate, and 7 parts of gelatin were weighed, wherein the mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion was 0.9:1.

[0065] (3) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water is 35% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1;

[0066] (4) The pH of the mixed material 1 was adjusted to 4 with a 2 mol / L phosphoric acid solution, and aluminum sulfate and gelatin were added thereto. The mixture was stirred at 250 r / min for 60 min at 85° C. to prepare a weather-resistant adhesive.

[0067] The untreated shear strength of the adhesive prepared in Comparative Example 3 is 3.59 MPa, the re-dry strength after immersion in hot water at 63°C for 3 hours is 3.44 MPa, and the re-dry strength after immersion in hot water at 93°C for 3 hours is 3.16 MPa. The test results show that the preparation method of the modified bio-based material is beneficial to improving the reactivity of lignin. In Comparative Example 3, the heating rate and reaction temperature are increased. During the heating modification process of lignin, active groups such as aromatic groups, phenolic hydroxyl groups, and alcoholic hydroxyl groups in the lignin molecular structure participate in the reaction. Excessively high heating rate and reaction temperature lead to the production of a variety of volatile compounds and non-volatile solids. The reactive groups of the modified bio-based material are reduced, and impurities are increased, resulting in a decrease in the use effect of the adhesive.

[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A weather-resistant adhesive, characterized in that: The raw materials include 50-70 parts of modified bio-based materials, 20-25 parts of styrene-acrylic emulsion, 0.5-1 parts of aluminum sulfate and 5-9 parts of gelatin by weight. The preparation method of the modified bio-based materials is to mix lignin, a metal catalyst and water, and react them at 500-600°C for 6-8h under a nitrogen atmosphere to obtain the modified bio-based materials. The metal catalyst is a nickel salt, and the mass ratio of the lignin, the metal catalyst and the water is 1:0.1-0.2:100-150.

2. The weather-resistant adhesive according to claim 1, characterized in that: The nitrogen pressure is 0.3-0.7Mpa.

3. The weather-resistant adhesive according to claim 1, characterized in that: The mass ratio of styrene to isooctyl acrylate in the styrene-acrylic emulsion is 0.8-1:

1.

4. The method for preparing the weather-resistant adhesive according to claim 1, characterized in that: The following steps are involved: (1) mixing water, styrene acrylic emulsion and modified bio-based material, wherein the amount of water is 30-40% of the total mass of the styrene acrylic emulsion and the modified bio-based material, to prepare a mixed material 1; (2) The pH value of the mixed material 1 is adjusted to 3-5, and aluminum sulfate and gelatin are added thereto, and the mixture is stirred at 200-300 r / min for 50-70 min at 80-90° C. to prepare a weather-resistant adhesive.

5. Use of the weather-resistant adhesive according to any one of claims 1 to 3 in bonding metal, plastic and wooden substrates.