A kind of high thermal conductivity aluminum alloy material and preparation method thereof
By using aluminum fluoride and sodium sulfate in aluminum alloy to reduce the viscosity of borax and adding composite metals of erbium and yttrium combined with silicon impurities, the problem of iron and silicon impurities in aluminum alloys affecting thermal conductivity is solved, and high conductivity and thermal conductivity are achieved Preparation of aluminium alloy materials.
Patent Information
- Application Number
- CN202410646805.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-05-23
AI Technical Summary
The iron and silicon impurities present in aluminum alloys will hinder the conduction of thermal conductivity and affect thermal conductivity. The existing borax flux has low iron removal efficiency and high viscosity, making it difficult to effectively remove impurities, and the high solid solubility of silicon affects the conductivity.
Aluminum fluoride and sodium sulfate are used as impurities to reduce the viscosity of borax and improve its fluidity. By adding composite metals of erbium and yttrium and combining with silicon impurities, the grains are refined to achieve iron removal and improve conductivity.
The conductivity and thermal conductivity of aluminum alloys are improved, and the conductive properties and heat resistance of the material are improved by effectively removing iron impurities and refining grains.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aluminum alloy processing and relates to a high thermal conductivity aluminum alloy material and a preparation method thereof. Background Art
[0002] Fe is one of the most important impurities in aluminum. The use of steel or cast iron tools for smelting and casting will bring Fe into aluminum, and Fe may be mixed into the scrap when remelting. The Fe content of the alloy recycled for multiple times will gradually increase. Fe has a negative impact on the electrical conductivity of cast aluminum, because it usually appears as coarse primary crystals or along primary crystals, or exists in the form of A1-Fe-Si compounds. The common iron phases in aluminum are α-A18SiFe2 phase and β-A15FeSi phase. Among them, the β-Fe phase is the main harmful phase to aluminum alloys. In addition, the presence of iron will lead to an increase in grain boundaries or coarsening of grains. These factors will hinder the conduction of heat, thereby affecting the overall thermal conductivity.
[0003] Current research has found that borax flux has a high potential for capturing Fe atoms, so boron compound flux is theoretically a feasible method for separating iron impurities from aluminum alloy melts. However, the high viscosity and agglomeration of borax compounds for iron removal greatly reduce the possibility of the flux contacting and reacting with the iron impurities in the melt, so the iron removal efficiency is low.
[0004] Si is the second most abundant impurity in aluminum, mainly from silicon dioxide or silicate in bauxite. The solid solubility of Si is greater than that of Fe. The solid solubility is 1.65% at the eutectic temperature of 577°C and 0.05% at room temperature. The influence of impurities in the solid solution state on the resistivity of the conductor is greater than that in the precipitation state. Therefore, Si as a basic impurity element has a much greater influence on the resistivity than Fe, and is the most important impurity element affecting the conductivity of aluminum conductors. In addition, the presence of silicon will significantly affect the thermal conductivity of aluminum alloys. The addition of silicon will reduce the thermal conductivity of aluminum alloys. This is related to the low thermal conductivity of silicon itself.
[0005] Therefore, in order to solve the above problems, the present invention provides a method for preparing a high thermal conductivity aluminum alloy material, by which an aluminum alloy material with good electrical conductivity and good thermal conductivity can be obtained. Summary of the invention
[0006] The present invention relates to a high thermal conductivity aluminum alloy material and a preparation method thereof, and belongs to the technical field of aluminum alloy processing. The present invention discloses a preparation method of a high thermal conductivity aluminum alloy material, which includes the following processes: raw material melting - adding an impurity remover to remove impurities - adding a composite metal - permanent magnetic stirring - cooling to obtain a high thermal conductivity aluminum alloy material. The present invention adds an iron remover to remove iron impurities in the raw material, wherein the aluminum fluoride and sodium sulfate in the iron remover reduce the viscosity of borax, thereby improving its fluidity and better contact with the iron impurities in the raw material to achieve the purpose of removing iron; at the same time, the addition of a composite metal composed of erbium and yttrium can be combined with silicon impurities in the raw material for precipitation, and has the effect of refining the grains of the aluminum material, so that an aluminum alloy material with high conductivity and heat resistance can be obtained.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A method for preparing a high thermal conductivity aluminum alloy material, the method for preparing a high thermal conductivity aluminum alloy material comprising the following steps:
[0009] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0010] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0011] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0012] (4) Mixture b is heated and melted, and the composite metal is added and stirred and mixed, and then cooled to obtain a high thermal conductivity aluminum alloy material.
[0013] The heating temperature in the step (1) is 750-800° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:20-30.
[0014] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 30-40 minutes.
[0015] The impurity remover in step (2) is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 5-6:1-2:1-2, the mass ratio of the aluminum ingot material to the impurity remover is 1-3:0.1-0.5, and the standing time is 20-30 minutes.
[0016] The insulation time and temperature in step (3) are 40-60 minutes and 700-750°C respectively, and the cooling refers to cooling to 50-60°C.
[0017] The mass concentration of the sodium hydroxide solution in step (3) is 10-15%, and the solid-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2-3 g / mL.
[0018] The melting temperature in step (4) is 700-750° C., and the mass ratio of the composite metal to the mixture b is 1:10-16, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:1.
[0019] The stirring time in step (4) is 1-2 hours, and the cooling refers to cooling to room temperature.
[0020] Beneficial effects of the present invention:
[0021] 1. Aluminum fluoride in the impurity remover can combine with borax to reduce the concentration of borax and increase its viscosity. At the same time, sodium sulfate can decompose into gas to increase the fluidity of borax and promote the combination with impurity iron in aluminum ingots to achieve the purpose of removing iron;
[0022] 2. Adding a composite metal composed of erbium and yttrium, erbium can combine with silicon impurities in the raw materials to precipitate, thereby reducing resistivity and improving electrical and thermal conductivity. At the same time, yttrium can refine the secondary dendrite structure of the alloy and reduce the size of the eutectic compound, that is, it has the effect of refining the grains of aluminum, further improving the electrical conductivity of the aluminum alloy material. DETAILED DESCRIPTION
[0023] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with embodiments.
[0024] Example 1
[0025] A method for preparing a high thermal conductivity aluminum alloy material, the method for preparing a high thermal conductivity aluminum alloy material comprising the following steps:
[0026] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0027] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0028] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0029] (4) Mixture b is heated and melted, and the composite metal is added and stirred and mixed, and then cooled to obtain a high thermal conductivity aluminum alloy material.
[0030] The heating temperature in the step (1) is 750° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:20.
[0031] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 30 minutes.
[0032] The impurity remover in step (2) is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 5:1:1, the mass ratio of the aluminum ingot material to the impurity remover is 1:0.1, and the standing time is 20 minutes.
[0033] The insulation time and temperature in step (3) are 40 minutes and 700° C. respectively, and the cooling refers to cooling to 50° C.
[0034] The mass concentration of the sodium hydroxide solution in step (3) is 10%, and the solid-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2 g / mL.
[0035] The melting temperature in step (4) is 700° C., and the mass ratio of the composite metal to the mixture b is 1:10, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:1.
[0036] The stirring time in step (4) is 1 hour, and the cooling refers to cooling to room temperature.
[0037] Example 2
[0038] A method for preparing a high thermal conductivity aluminum alloy material, the method for preparing a high thermal conductivity aluminum alloy material comprising the following steps:
[0039] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0040] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0041] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0042] (4) Mixture b is heated and melted, and the composite metal is added and stirred and mixed, and then cooled to obtain a high thermal conductivity aluminum alloy material.
[0043] The heating temperature in the step (1) is 780° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:25.
[0044] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 35 minutes.
[0045] The impurity remover in step (2) is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 5.5:1.5:1.5, the mass ratio of the aluminum ingot material to the impurity remover is 2:0.3, and the standing time is 25 minutes.
[0046] The insulation time and temperature in step (3) are 50 min and 720° C. respectively, and the cooling refers to cooling to 55° C.
[0047] The mass concentration of the sodium hydroxide solution in step (3) is 13%, and the solid-to-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2.5 g / mL.
[0048] The melting temperature in step (4) is 720° C., and the mass ratio of the composite metal to the mixture b is 1:13, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:1.
[0049] The stirring time in step (4) is 1.5 h, and the cooling refers to cooling to room temperature.
[0050] Example 3
[0051] A method for preparing a high thermal conductivity aluminum alloy material, the method for preparing a high thermal conductivity aluminum alloy material comprising the following steps:
[0052] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0053] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0054] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0055] (4) Mixture b is heated and melted, and the composite metal is added and stirred and mixed, and then cooled to obtain a high thermal conductivity aluminum alloy material.
[0056] The heating temperature in the step (1) is 800° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:30.
[0057] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 40 minutes.
[0058] The impurity remover in step (2) is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 6:2:2, the mass ratio of the aluminum ingot material to the impurity remover is 3:0.5, and the standing time is 30 minutes.
[0059] The insulation time and temperature in step (3) are 60 minutes and 750° C. respectively, and the cooling refers to cooling to 60° C.
[0060] The mass concentration of the sodium hydroxide solution in step (3) is 15%, and the solid-liquid ratio of the mixture a to the sodium hydroxide solution is 10:3 g / mL.
[0061] The melting temperature in step (4) is 750° C., and the mass ratio of the composite metal to the mixture b is 1:16, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:1.
[0062] The stirring time in step (4) is 2 hours, and the cooling refers to cooling to room temperature.
[0063] Comparative Example 1
[0064] Based on Example 2, a method for preparing a high thermal conductivity aluminum alloy material is provided, and the method for preparing a high thermal conductivity aluminum alloy material comprises the following steps:
[0065] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0066] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0067] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0068] (4) Mixture b is heated and melted, and the composite metal is added and stirred and mixed, and then cooled to obtain a high thermal conductivity aluminum alloy material.
[0069] The heating temperature in the step (1) is 780° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:25.
[0070] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 35 minutes.
[0071] The impurity remover in step (2) is composed of borax and sodium sulfate in a mass ratio of 5.5:1.5, the mass ratio of the aluminum ingot material to the impurity remover is 2:0.3, and the standing time is 25 minutes.
[0072] The insulation time and temperature in step (3) are 50 min and 720° C. respectively, and the cooling refers to cooling to 55° C.
[0073] The mass concentration of the sodium hydroxide solution in step (3) is 13%, and the solid-to-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2.5 g / mL.
[0074] The melting temperature in step (4) is 720° C., and the mass ratio of the composite metal to the mixture b is 1:13, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:1.
[0075] The stirring time in step (4) is 1.5 h, and the cooling refers to cooling to room temperature.
[0076] Comparative Example 2
[0077] Based on Example 2, a method for preparing a high thermal conductivity aluminum alloy material is provided, and the method for preparing a high thermal conductivity aluminum alloy material comprises the following steps:
[0078] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0079] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0080] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0081] (4) Mixture b is heated and melted, and the composite metal is added and stirred and mixed, and then cooled to obtain a high thermal conductivity aluminum alloy material.
[0082] The heating temperature in the step (1) is 780° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:25.
[0083] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 35 minutes.
[0084] The impurity remover in step (2) is composed of borax and aluminum fluoride in a mass ratio of 5.5:1.5, the mass ratio of the aluminum ingot material to the impurity remover is 2:0.3, and the standing time is 25 minutes.
[0085] The insulation time and temperature in step (3) are 50 min and 720° C. respectively, and the cooling refers to cooling to 55° C.
[0086] The mass concentration of the sodium hydroxide solution in step (3) is 13%, and the solid-to-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2.5 g / mL.
[0087] The melting temperature in step (4) is 720° C., and the mass ratio of the composite metal to the mixture b is 1:13, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:1.
[0088] The stirring time in step (4) is 1.5 h, and the cooling refers to cooling to room temperature.
[0089] Comparative Example 3
[0090] Based on Example 2, a method for preparing a high thermal conductivity aluminum alloy material is provided, and the method for preparing a high thermal conductivity aluminum alloy material comprises the following steps:
[0091] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0092] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0093] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0094] (4) Mixture b is heated and melted, metal is added and stirred, and after cooling, a high thermal conductivity aluminum alloy material is obtained.
[0095] The heating temperature in the step (1) is 780° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:25.
[0096] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 35 minutes.
[0097] The impurity remover in step (2) is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 5.5:1.5:1.5, the mass ratio of the aluminum ingot material to the impurity remover is 2:0.3, and the standing time is 25 minutes.
[0098] The insulation time and temperature in step (3) are 50 min and 720° C. respectively, and the cooling refers to cooling to 55° C.
[0099] The mass concentration of the sodium hydroxide solution in step (3) is 13%, and the solid-to-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2.5 g / mL.
[0100] The melting temperature in step (4) is 720° C., the mass ratio of the metal to the mixture b is 1:13, and the metal is erbium.
[0101] The stirring time in step (4) is 1.5 h, and the cooling refers to cooling to room temperature.
[0102] Comparative Example 4
[0103] Based on Example 2, a method for preparing a high thermal conductivity aluminum alloy material is provided, and the method for preparing a high thermal conductivity aluminum alloy material comprises the following steps:
[0104] (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand;
[0105] (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a;
[0106] (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b.
[0107] (4) Mixture b is heated and melted, metal is added and stirred, and after cooling, a high thermal conductivity aluminum alloy material is obtained.
[0108] The heating temperature in the step (1) is 780° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:25.
[0109] In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 35 minutes.
[0110] The impurity remover in step (2) is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 5.5:1.5:1.5, the mass ratio of the aluminum ingot material to the impurity remover is 2:0.3, and the standing time is 25 minutes.
[0111] The insulation time and temperature in step (3) are 50 min and 720° C. respectively, and the cooling refers to cooling to 55° C.
[0112] The mass concentration of the sodium hydroxide solution in step (3) is 13%, and the solid-to-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2.5 g / mL.
[0113] The melting temperature in step (4) is 720° C., the mass ratio of the metal to the mixture b is 1:13, and the metal is yttrium.
[0114] The stirring time in step (4) is 1.5 h, and the cooling refers to cooling to room temperature.
[0115] Performance Testing
[0116] 1. The aluminum alloy materials prepared in Example 2 and Comparative Examples 1-4 were used as samples, and their thermal conductivity and electrical conductivity were tested according to GB / T 22588-2008 "Flash method for measurement of thermal diffusivity or thermal conductivity" and GB / T 12966-2022 "Eddy current test method for electrical conductivity of aluminum and aluminum alloys".
[0117] The above test results are shown in Table 1.
[0118] Table 1 Test results
[0119] Sample Thermal conductivity / (W / (m*K)) Electrical conductivity / %IACS Example 2 179.3 63.78 Comparative Example 1 152.6 42.13 Comparative Example 2 162.0 43.01 Comparative Example 3 159.4 50.21 Comparative Example 4 157.0 52.13
[0120] From the data analysis in Table 1, it can be concluded that the thermal conductivity and electrical conductivity of Example 2 are greater than those of Comparative Examples 1-4. The stronger the thermal conductivity of a thermal conductivity material, the greater the intensity of heat transfer, and the better the thermal conductivity of the material. Comparative Examples 1-2 did not add sodium sulfate or aluminum fluoride, and due to the influence of borax viscosity, the removal of iron decreased, thereby reducing the thermal conductivity and electrical conductivity; Comparative Examples 3-4 did not add erbium or yttrium, and their thermal conductivity and electrical conductivity decreased.
[0121] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a high thermal conductivity aluminum alloy material, It is characterized in that The preparation method of the high thermal conductivity aluminum alloy material comprises the following steps: (1) heating the aluminum ingot material to melt it, adding a refining agent and allowing it to stand; (2) then adding an impurity remover, stirring and mixing, and allowing to stand to form a mixture a; The impurity remover is composed of borax, aluminum fluoride and sodium sulfate in a mass ratio of 5-6:1-2:1-2; the mass ratio of the aluminum ingot material to the impurity remover is 1-3:0.1-0.5; (3) transferring the mixture a into a crucible and allowing it to settle at a temperature of 100 °C. After cooling, adding a sodium hydroxide solution, removing the solution, and washing with ethanol to obtain a mixture b. (4) heating the mixture b to melt, adding the composite metal, stirring and mixing, and cooling to obtain a high thermal conductivity aluminum alloy material; The mass ratio of the composite metal to the mixture b is 1:10-16, wherein the composite metal is composed of erbium and yttrium in a mass ratio of 1:
1.
2. A method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that The heating temperature in the step (1) is 750-800° C., and the mass ratio of the refining agent to the aluminum ingot material is 1:20-30.
3. The method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that In the step (1), the refining agent is composed of potassium chloride and sodium fluorosilicate in a mass ratio of 1:1, and the standing time is 30-40 minutes.
4. The method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that The standing time in step (2) is 20-30 minutes.
5. The method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that The insulation time and temperature in step (3) are 40-60 minutes and 700-750°C respectively, and the cooling refers to cooling to 50-60°C.
6. The method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that The mass concentration of the sodium hydroxide solution in step (3) is 10-15%, and the solid-liquid ratio of the mixture a to the sodium hydroxide solution is 10:2-3 g / mL.
7. The method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that The melting temperature in step (4) is 700-750°C.
8. The method for preparing a high thermal conductivity aluminum alloy material according to claim 1, It is characterized in that The stirring time in step (4) is 1-2 hours, and the cooling refers to cooling to room temperature.
Citation Information
Patent Citations
Heat-resistant aluminum alloy conductor material with electric conductivity of 62 percent and preparation method for heat-resistant aluminum alloy conductor material
CN104561674A
Iron removal method for regenerated Al-Cu-Si series aluminum alloy
CN107619959A
Low-iron low-silicon aluminum liquid and preparation method and application thereof
CN113106282A
High-elongation aluminum alloy and preparation method thereof
CN114855033A
Aluminum alloy refining agent for removing iron and heat treatment process of aluminum alloy refining agent
CN115161506A