A high temperature resistant and high thermal conductivity insulating casting adhesive and preparation method thereof
By using boron nitride and alumina as thermal fillers in epoxy resin and preparing flame retardant epoxy resin through reaction of specific components, the problems of low thermal conductivity and insufficient thermal resistance of epoxy resin are solved, and the problem of low thermal conductivity and insufficient thermal resistance of epoxy resin is achieved. High thermal conductivity and high temperature resistance casting glue improves the reliability and service life of the product.
Patent Information
- Application Number
- CN202410560423.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-05-08
AI Technical Summary
The thermal conductivity of epoxy resin is low, affecting the heat dissipation of the equipment, and its heat resistance needs to be further improved to ensure the reliability and service life of the product.
Boron nitride and alumina are used as thermal fillers to form a casting glue with high thermal conductivity and high temperature resistance through crosslinking with epoxy resin. The flame-retardant epoxy resin is prepared by using melamine, dibenzaldehyde, diamine and other components. , enhance its thermal stability, and improve the dispersion and adhesion of thermal filler through surface modification.
The thermal conductivity, high temperature resistance and flame retardant properties of cast glue are significantly improved, ensuring its stability and mechanical properties under high temperature conditions.
Smart Images

Figure BDA0004827539830000101 
Figure BDA0004827539830000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of epoxy resin casting, in particular to a high-temperature resistant and high-thermal conductive insulating casting adhesive and a preparation method thereof. Background Art
[0002] As a thermosetting resin, epoxy resin has good mechanical properties, dimensional stability and electrical insulation properties, and is widely used in electronic packaging fields such as adhesives, casting materials, and coatings. The molecular structure of epoxy resin contains active epoxy groups, which can undergo a cross-linking reaction with the curing agent to form a polymer with a three-dimensional network structure. After curing, it can form a good bond with the conductor material and has a good insulation effect. However, the thermal conductivity of epoxy resin is low, which is not conducive to the heat dissipation of equipment, and overheating will have a serious impact on the reliability and service life of the product. And the heat resistance of epoxy resin needs to be further improved. Therefore, we propose a high temperature resistant and high thermal conductivity insulating casting adhesive and a preparation method thereof. Summary of the invention
[0003] The object of the present invention is to provide a high temperature resistant and high thermal conductivity insulating casting adhesive and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0004] In order to solve the above technical problems, the present invention provides the following technical solution: a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following mass components: 60 to 80 parts of epoxy resin, 20 to 40 parts of flame retardant epoxy resin, 10 to 30 parts of thermal conductive filler, 8 to 10 parts of flame retardant filler, 6 to 10 parts of plasticizer, 74 to 85 parts of curing agent and 0.5 to 2.0 parts of accelerator.
[0005] Furthermore, the epoxy resin is bisphenol A epoxy resin or bisphenol F epoxy resin.
[0006] Furthermore, the thermally conductive filler is a mixture of two or more of aluminum oxide, aluminum nitride, silicon carbide, zinc oxide, and boron nitride.
[0007] Furthermore, the thermally conductive filler is boron nitride and aluminum oxide, and the mass ratio is (1.7-3.0):1.
[0008] Furthermore, the flame retardant filler is one of aluminum hydroxide and magnesium hydroxide, or a mixture of the two.
[0009] Furthermore, the curing agent is one of toluene tetrahydrophthalic anhydride, 2,3,3',4'-diphenyl ether tetracarboxylic dianhydride, 1,2,3,4-cyclopentanetetracarboxylic dianhydride, tetrachlorophthalic anhydride, 4,4'-diaminodiphenylmethane, and 4,4'-diaminodiphenyl sulfone.
[0010] Furthermore, the accelerator is one of N,N-dimethylbenzylamine and 1,2-dimethylimidazole.
[0011] In the above technical scheme, boron nitride has a graphite-like crystal structure, excellent thermal conductivity, high temperature resistance and good electrical insulation performance, and is an ideal thermal conductive filling material. The nano-sheet structure of boron nitride and its surface polarity can interact with the resin system, thereby improving its dispersibility and adhesion in the casting glue, and improving the mechanical properties of the casting glue solid. Alumina has a narrow particle size distribution, good dimensional stability, and good thermal conductivity. It can be filled in the resin system in large quantities to form a thermal conductive path in the casting glue system, so that the prepared casting glue solid has better thermal conductivity and thermal diffusion ability. At the same time, the casting glue can also maintain good fluidity and will not hinder the processing performance of the casting glue. Therefore, boron nitride and aluminum oxide are selected as thermal conductive fillers for casting glue. The filling of flaky and spherical fillers in epoxy resin can construct thermal conductive paths in the horizontal and vertical directions, which is helpful for the realization of high thermal conductivity of the casting glue solid.
[0012] A method for preparing a high-temperature resistant and high-thermal conductive insulating casting adhesive comprises the following processes: mixing epoxy resin with flame-retardant epoxy resin, plasticizer, thermal conductive filler and flame-retardant filler in sequence, adding a curing agent and an accelerator, and dispersing them evenly to obtain a casting adhesive.
[0013] Furthermore, the flame retardant epoxy resin is prepared by the following process:
[0014] S1. Mix dibenzaldehyde and anhydrous ethanol, heat to 50-60°C, stir and add melamine, heat to 85-90°C, continue stirring, and keep warm for reflux reaction for 8-10 hours; filter and wash with methanol, and vacuum dry at 70-75°C to obtain an aldehyde compound;
[0015] S2, mixing the aldehyde compound, diamine and anhydrous ethanol, heating to 60-75°C, stirring and keeping the temperature under reflux for 3-5h; adding DOPO, heating to 85-95°C, reacting for 16-18h; cooling to room temperature, filtering, washing, and vacuum drying at 60-65°C to obtain an amino compound;
[0016] S3, mixing the amino compound, alkenyl silane and anhydrous toluene, heating to 100-110° C., reacting for 2-4 hours; washing, drying, and obtaining an alkenyl compound;
[0017] S4. Mix the alkenyl compound and chloroform, add glacial acetic acid and concentrated sulfuric acid, stir and heat to 70-80°C, slowly add hydrogen peroxide, and reflux for 6-8h; wash and dry to obtain a flame-retardant epoxy resin.
[0018] Further, in step S1, the molar ratio of melamine to benzaldehyde is 1:(3.0-3.1);
[0019] The ratio of benzaldehyde to anhydrous ethanol is 30 g / 100 mL;
[0020] Melamine was added in the form of an anhydrous ethanol solution.
[0021] Further, in step S1, the benzaldehyde is 4-(4-formylphenoxy)benzaldehyde, 2,2'-oxybenzaldehyde, 4,4'-diformyltriphenylamine, 2,7-benzaldehyde-benzothiadiazole, 9,10-di(4-formylphenyl)anthracene, 4,4'-(pyrene-1,6-diyl)benzaldehyde, 4,4'-(naphthalene-1,4-diyl)benzaldehyde, 4,4-(piperazine-1,4-diyl)benzaldehyde, 2, One of 9-bis[P-(formyl)phenyl]-1,10-phenanthroline, 4,4'-(1,10-phenanthroline-3,8-diyl)benzaldehyde, 4,4'-([2,2'-bipyridine]-5,5'-diyl)benzaldehyde, 4,4'-(1H-benzo[D]imidazole-4,7-diyl)benzaldehyde, and 4,4'-[biphenyl-4,4'-diylbis(1-naphthalen-1-ylazadiyl)]benzaldehyde.
[0022] Further, in step S2, the molar ratio of the aldehyde compound to the diamine is 1:(3.01-3.20);
[0023] The ratio of aldehyde compound and anhydrous ethanol is 15 g / 100 mL;
[0024] The mass ratio of DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) is 15:(2-4).
[0025] Furthermore, in step S2, the diamine is one of 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane, 1,2-diaminocyclohexane, and 1,6-hexanediamine.
[0026] Further, in step S3, the molar ratio of the amino compound to the alkenyl silane is 1:(3.01-3.20);
[0027] The ratio of the amino compound to anhydrous toluene was 15 g / 100 mL.
[0028] Furthermore, in step S3, the alkenyl silane is one or a mixture of trivinyltrimethylcyclotrisilazane and 2,4,6-trivinyl-2,4,6-trimethylcyclotrisiloxane.
[0029] Further, in step S4, the ratio of the alkenyl compound to chloroform is 5 g / 100 mL;
[0030] The ratio of the olefin compound, glacial acetic acid, concentrated sulfuric acid, and hydrogen peroxide is 5 g: (38-45) mL: (1.6-2.2) mL: (80-100) mL.
[0031] In the above technical scheme, the flame-retardant epoxy resin is obtained by reacting components such as melamine, benzaldehyde, diamine, and alkenyl silane. According to the synthesis order of the reactants, melamine is first reacted with benzaldehyde, and then diamine is added, so that the two groups of aldehyde groups in benzaldehyde are sequentially condensed with the amino groups in melamine and diamine to form imine bonds, which can react with the phosphorus-hydrogen bonds of DOPO in the subsequent reaction process to connect phosphorus to the molecular chain of the flame-retardant epoxy resin, and cooperate with the nitrogen heterocycle in melamine and the rigid ring structure in diamine, which significantly improves the thermal stability of the epoxy resin system, so that the prepared casting glue cured product has excellent high temperature resistance, flame retardant properties and mechanical properties. Then the obtained amino compound is added with alkenyl silane to obtain an alkenyl compound, and the alkenyl group is epoxidized to form a flame-retardant epoxy resin. The alkenyl silanes selected are trivinyltrimethylcyclotrisilazane and trivinyltrimethylcyclotrisiloxane. The cyclic silanes can further improve the heat resistance temperature and thermal stability of the flame retardant epoxy resin. The participation of trifunctional reactants is helpful to improve the fluidity and curing crosslinking degree of the epoxy resin system, thereby effectively improving the heat resistance, flame retardancy and mechanical properties of the prepared casting adhesive.
[0032] Furthermore, the thermally conductive filler is surface-modified.
[0033] Further, the surface modification process of boron nitride is as follows:
[0034] Boron nitride, dopamine hydrochloride, Tris buffer and ethanol are mixed, and ultrasonically dispersed for 20 to 30 minutes; stirred for reaction for 12 hours; heated to 80 to 90° C., an amino compound is added, and stirred for reaction at a speed of 1000 to 1500 rpm for 6 to 8 hours; cooled, filtered, washed, and dried at 80 to 85° C. to obtain modified boron nitride.
[0035] Furthermore, the ratio of boron nitride, dopamine hydrochloride, amino compound, Tris buffer (trishydroxymethylaminomethane), and ethanol is 10 g: (10-13) g: (1.5-2.5) g: 100 mL: (35-40) mL.
[0036] In the above technical scheme, dopamine is polymerized on the surface of boron nitride to coat it, and then the amino compound prepared above is added for modification, so that a high-temperature resistant and rigid structure is loaded on the surface of boron nitride, which helps to improve the interfacial thermal resistance between it and the epoxy resin, promote the construction of a thermal conductive path in the casting glue, and improve the thermal conductivity, high-temperature resistance and mechanical properties of its cured product.
[0037] Further, the surface modification process of alumina is as follows:
[0038] Mix alumina and acetone, add KH-560, stir for 60-75 minutes, place at 60-65°C, continue stirring for 3-4 hours; cool, wash, and dry at 80-85°C to obtain modified alumina.
[0039] Furthermore, the ratio of alumina, KH-560 (γ-glycidyloxypropyltrimethoxysilane) and acetone is 2 g: (0.1-0.2) g: 100 mL.
[0040] In the above technical scheme, the coupling modification of alumina by using γ-glycidyloxypropyltrimethoxysilane can improve the dispersibility of alumina in epoxy resin. At the same time, the epoxy groups on the surface of the modified alumina can react with the amino groups on the surface of the curing agent and the modified boron chloride, thereby improving the crosslinking degree in the casting glue curing system, which is helpful to further improve its mechanical properties and high temperature resistance.
[0041] An application of a high temperature resistant and high thermal conductivity insulating casting adhesive is used in the field of electronic packaging casting; the casting adhesive is injected into the area to be cast and solidified.
[0042] Furthermore, the curing process conditions are: keep warm at 60-80°C for 30 minutes; heat up to 100-120°C and keep warm for 2-3 hours; heat up to 140-160°C and keep warm for 2-3 hours; cool down to 120-140°C and keep warm for 1-2 hours; cool down to 80-100°C and keep warm for 1-2 hours;
[0043] Before curing, place in a 45-50℃ oven for vacuum degassing.
[0044] Compared with the prior art, the present invention has the following beneficial effects:
[0045] The high-temperature and high-thermal-conductivity insulating casting adhesive described in the present invention selects boron nitride and aluminum oxide as thermally conductive fillers of the casting adhesive, and fills flaky and spherical fillers in the epoxy resin, so as to construct thermal conductive paths in the horizontal and vertical directions, which is helpful to achieve high thermal conductivity of the casting adhesive cured product; the flame-retardant epoxy resin is prepared by reacting components such as melamine, dibenzaldehyde, diamine, alkenyl silane, DOPO, etc., which can significantly improve the thermal stability of the epoxy resin system, so that the prepared casting adhesive cured product has excellent high temperature resistance, flame retardant properties and mechanical properties. DETAILED DESCRIPTION
[0046] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] In the following specific implementations:
[0048] Boron nitride: Hexagonal boron nitride (h-BN): flake diameter 5-10 μm, from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0049] Alumina: Nano-alumina (Al2O3): spherical, particle size 20-30 nm, sourced from Beijing Dekedaojin Technology Co., Ltd.;
[0050] Aluminum hydroxide: particle size 25 μm, from Shanghai MacLean Biochemical Technology Co., Ltd.;
[0051] Magnesium hydroxide: H1410, from Weifang Haililong Magnesium Industry Co., Ltd.;
[0052] Epoxy resin: E-44, from Henan Zepu Chemical Products Co., Ltd.;
[0053] The plasticizer is dioctyl phthalate; the curing agent is 4,4'-diaminodiphenylmethane; the accelerator is 1,2-dimethylimidazole;
[0054] The following “parts” are all parts by mass.
[0055] Embodiment 1: A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following process:
[0056] Step 1, preparation of flame retardant epoxy resin:
[0057] S1. Mix 30g of 2,7-dibenzaldehyde-benzothiadiazole and 100mL of anhydrous ethanol, heat to 50°C, stir and add melamine, heat to 85°C, continue stirring, and keep the temperature under reflux for 10 hours; filter and wash with methanol, and vacuum dry at 70°C to obtain an aldehyde compound; the molar ratio of melamine to 2,7-dibenzaldehyde-benzothiadiazole is 1:3;
[0058] S2. Mix 15 g of aldehyde compound, 10 g of 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane and 100 mL of anhydrous ethanol, heat to 60°C, stir and reflux for 5 h; add 16.6 g of DOPO, heat to 85°C, react for 18 h; cool to room temperature, filter, wash, and vacuum dry at 60°C to obtain an amino compound;
[0059] S3, 15 g of the amino compound, 3.7 g of trivinyltrimethylcyclotrisilazane and 100 mL of anhydrous toluene were mixed, the temperature was raised to 100° C., and the mixture was reacted for 4 h; the mixture was washed and dried to obtain an alkenyl compound;
[0060] S4, 5g of alkenyl compound and 100mL of chloroform were mixed, 38mL of glacial acetic acid and 1.6mL of concentrated sulfuric acid were added, stirred and heated to 70°C, 80mL of hydrogen peroxide was slowly added, and refluxed for 6-8h; washed and dried to obtain a flame-retardant epoxy resin;
[0061] Step 2: Surface modification of boron nitride:
[0062] 10g of boron nitride, 10g of dopamine hydrochloride, 100mL of Tris buffer and 35mL of ethanol were mixed and ultrasonically dispersed for 20min; stirred and reacted for 12h; the temperature was raised to 80-90℃, 1.5g of amino compound was added, and stirred and reacted at a speed of 1000rpm for 8h; cooled, filtered, washed, and dried at 80℃ to obtain modified boron nitride;
[0063] Step 3: Surface modification of alumina:
[0064] Mix 2g of alumina and 100mL of acetone, add 0.1g of KH-560, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified alumina;
[0065] Step 4: Preparation of casting glue:
[0066] 80 parts of epoxy resin are mixed in sequence with 20 parts of flame retardant epoxy resin, 6 parts of plasticizer, 10 parts of thermal conductive filler (modified boron nitride and modified alumina in a mass ratio of 1.7:1), and 8 parts of flame retardant filler (aluminum hydroxide and magnesium hydroxide in a mass ratio of 1.5:1), 74 parts of curing agent and 0.5 part of accelerator are added, and dispersed evenly to obtain a casting glue.
[0067] Embodiment 2: A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following process:
[0068] Step 1, preparation of flame retardant epoxy resin:
[0069] S1. Mix 30 g of 4,4-(piperazine-1,4-diyl)benzaldehyde and 100 mL of anhydrous ethanol, heat to 55°C, stir and add melamine, heat to 88°C, continue stirring, and keep warm for 9 hours of reflux reaction; filter and wash with methanol, and vacuum dry at 72°C to obtain an aldehyde compound; the molar ratio of melamine to 4,4-(piperazine-1,4-diyl)benzaldehyde is 1:3.05;
[0070] S2. Mix 15 g of aldehyde compound, 12.1 g of 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane and 100 mL of anhydrous ethanol, heat to 68°C, stir and keep reflux for 3 to 5 hours; add 19.3 g of DOPO, heat to 90°C, react for 17 hours; cool to room temperature, filter, wash, and vacuum dry at 62°C to obtain an amino compound;
[0071] S3, 15g of the amino compound, 4.0g of 2,4,6-trivinyl-2,4,6-trimethylcyclotrisiloxane and 100mL of anhydrous toluene were mixed, the temperature was raised to 105°C, and the reaction was performed for 3h; the mixture was washed and dried to obtain an alkenyl compound;
[0072] S4, 5g of alkenyl compound and 100mL of chloroform were mixed, 42mL of glacial acetic acid and 2mL of concentrated sulfuric acid were added, stirred and heated to 75°C, 90mL of hydrogen peroxide was slowly added, and refluxed for 7h; washed and dried to obtain a flame-retardant epoxy resin;
[0073] Step 2: Surface modification of boron nitride:
[0074] 10 g of boron nitride, 11 g of dopamine hydrochloride, 100 mL of Tris buffer and 38 mL of ethanol were mixed and ultrasonically dispersed for 25 min; stirred and reacted for 12 h; the temperature was raised to 85 ° C, 2 g of amino compound was added, and the reaction was stirred at a speed of 1200 rpm for 7 h; cooled, filtered, washed, and dried at 82 ° C to obtain modified boron nitride;
[0075] Step 3: Surface modification of alumina:
[0076] Mix 2g of alumina and 100mL of acetone, add 0.15g of KH-560, stir for 68min, place at 62°C, and continue stirring for 35h; cool, wash, and dry at 80-85°C to obtain modified alumina;
[0077] Step 4: Preparation of casting glue:
[0078] 80 parts of epoxy resin are mixed in sequence with 20 parts of flame retardant epoxy resin, 8 parts of plasticizer, 20 parts of thermal conductive filler (modified boron nitride and modified alumina in a mass ratio of 2.5:1), and 9 parts of flame retardant filler (aluminum hydroxide and magnesium hydroxide in a mass ratio of 2.4:1), and 80 parts of curing agent and 1.2 parts of accelerator are added and dispersed evenly to obtain a casting glue.
[0079] Embodiment 3: A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following process:
[0080] Step 1, preparation of flame retardant epoxy resin:
[0081] S1. Mix 30 g of 4,4'-(pyrene-1,6-diyl)benzaldehyde and 100 mL of anhydrous ethanol, heat to 60°C, stir and add melamine, heat to 90°C, continue stirring, and keep warm and reflux for 8 hours; filter and wash with methanol, and vacuum dry at 75°C to obtain an aldehyde compound; the molar ratio of melamine to 4,4'-(pyrene-1,6-diyl)benzaldehyde is 1:3.1;
[0082] S2, 15g of aldehyde compound, 8.5g of 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane and 100mL of anhydrous ethanol were mixed, the temperature was raised to 75°C, and the mixture was stirred and kept under reflux for 3h; 14.3g of DOPO was added, the temperature was raised to 95°C, and the mixture was reacted for 16h; the mixture was cooled to room temperature, filtered, washed, and dried under vacuum at 65°C to obtain an amino compound;
[0083] S3, 15g of the amino compound, 3.5g of trivinyltrimethylcyclotrisilazane and 100mL of anhydrous toluene were mixed, the temperature was raised to 110°C, and the reaction was performed for 2h; the mixture was washed and dried to obtain an alkenyl compound;
[0084] S4, 5g of alkenyl compound and 100mL of chloroform were mixed, 45mL of glacial acetic acid and 2.2mL of concentrated sulfuric acid were added, stirred and heated to 80°C, 100mL of hydrogen peroxide was slowly added, and refluxed for 6h; washed and dried to obtain a flame-retardant epoxy resin;
[0085] Step 2: Surface modification of boron nitride:
[0086] 10 g of boron nitride, 13 g of dopamine hydrochloride, 100 mL of Tris buffer and 40 mL of ethanol were mixed and ultrasonically dispersed for 30 min; stirred and reacted for 12 h; heated to 90 ° C, added 2.5 g of amino compound, stirred and reacted at a speed of 1500 rpm for 6 h; cooled, filtered, washed, and dried at 85 ° C to obtain modified boron nitride;
[0087] Step 3: Surface modification of alumina:
[0088] Mix 2g of alumina and 100mL of acetone, add 0.2g of KH-560, stir for 75min, place at 65℃, and continue stirring for 3h; cool, wash, and dry at 85℃ to obtain modified alumina;
[0089] Step 4: Preparation of casting glue:
[0090] Mix 80 parts of epoxy resin, 20 parts of flame retardant epoxy resin, 10 parts of plasticizer, 30 parts of thermal conductive filler (modified boron nitride and modified alumina in a mass ratio of 3:1), and 10 parts of flame retardant filler (aluminum hydroxide and magnesium hydroxide in a mass ratio of 3.3:1), add 85 parts of curing agent and 2.0 parts of accelerator, disperse evenly, and obtain casting glue.
[0091] Comparative Example 1: A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following processes:
[0092] Step 1, preparation of flame retardant epoxy resin:
[0093] Mix 15 g of melamine, 6.1 g of trivinyltrimethylcyclotrisilazane and 100 mL of anhydrous toluene, heat to 80° C., and react for 4 h; wash and dry to obtain an olefinic compound;
[0094] Mix 5g of alkenyl compound and 100mL of chloroform, add 38mL of glacial acetic acid and 1.6mL of concentrated sulfuric acid, stir and heat to 70°C, slowly add 80mL of hydrogen peroxide, reflux for 6-8h; wash and dry to obtain a flame-retardant epoxy resin;
[0095] Step 2: Surface modification of boron nitride:
[0096] Mix 2g of boron nitride and 100mL of acetone, add 0.1g of KH-550, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified boron nitride;
[0097] Step 3: Surface modification of alumina:
[0098] Mix 2g of alumina and 100mL of acetone, add 0.1g of KH-560, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified alumina;
[0099] Step 4: Preparation of casting glue:
[0100] 80 parts of epoxy resin are mixed in sequence with 20 parts of flame retardant epoxy resin, 6 parts of plasticizer, 10 parts of thermal conductive filler (modified boron nitride and modified alumina in a mass ratio of 1.7:1), and 8 parts of flame retardant filler (aluminum hydroxide and magnesium hydroxide in a mass ratio of 1.5:1), 70 parts of curing agent and 0.5 part of accelerator are added, and dispersed evenly to obtain a casting glue.
[0101] Comparative Example 2: A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following processes:
[0102] Step 1, preparation of flame retardant epoxy resin:
[0103] Mix 15 g of 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane, 46.4 g of trivinyltrimethylcyclotrisilazane and 100 mL of anhydrous toluene, heat to 80° C., and react for 4 h; wash and dry to obtain an olefinic compound;
[0104] Mix 5g of alkenyl compound and 100mL of chloroform, add 38mL of glacial acetic acid and 1.6mL of concentrated sulfuric acid, stir and heat to 70°C, slowly add 80mL of hydrogen peroxide, reflux for 6-8h; wash and dry to obtain a flame-retardant epoxy resin;
[0105] Step 2: Surface modification of boron nitride:
[0106] Mix 2g of boron nitride and 100mL of acetone, add 0.1g of KH-550, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified boron nitride;
[0107] Step 3: Surface modification of alumina:
[0108] Mix 2g of alumina and 100mL of acetone, add 0.1g of KH-560, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified alumina;
[0109] Step 4: Preparation of casting glue:
[0110] 80 parts of epoxy resin are mixed in sequence with 20 parts of flame retardant epoxy resin, 6 parts of plasticizer, 10 parts of thermal conductive filler (modified boron nitride and modified alumina in a mass ratio of 1.7:1), and 8 parts of flame retardant filler (aluminum hydroxide and magnesium hydroxide in a mass ratio of 1.5:1), 74 parts of curing agent and 0.5 part of accelerator are added, and dispersed evenly to obtain a casting glue.
[0111] Comparative Example 3: A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive, comprising the following processes:
[0112] Step 1: Surface modification of boron nitride:
[0113] Mix 2g of boron nitride and 100mL of acetone, add 0.1g of KH-550, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified boron nitride;
[0114] Step 2: Surface modification of alumina:
[0115] Mix 2g of alumina and 100mL of acetone, add 0.1g of KH-560, stir for 60min, place at 60℃, and continue stirring for 4h; cool, wash, and dry at 80-85℃ to obtain modified alumina;
[0116] Step 3: Preparation of casting glue:
[0117] 100 parts of epoxy resin (E-44) were mixed in sequence with 6 parts of plasticizer, 10 parts of thermal conductive filler (modified boron nitride and modified alumina in a mass ratio of 3:1), and 8 parts of flame retardant filler (aluminum hydroxide and magnesium hydroxide in a mass ratio of 1.5:1), and 74 parts of curing agent and 0.5 parts of accelerator were added and dispersed evenly to obtain a casting glue.
[0118] experiment
[0119] Take the flame-retardant epoxy resin obtained in Example 1-3 and Comparative Example 1-3 (mixed with the corresponding number of epoxy resins and curing agents) and the casting glue, cast, place in a 45°C oven for vacuum degassing, and cure. The curing conditions are: keep warm at 80°C for 30 minutes; heat to 120°C for 2 hours; heat to 160°C and keep warm for 2 hours; cool to 120°C and keep warm for 1 hour; cool to 80°C and keep warm for 1 hour to form epoxy resin cured products and casting glue cured products, and prepare samples; test their properties respectively and record the test results:
[0120] Thermal conductivity test: The thermal conductivity of the cast glue solidified sample was tested using a heat flow method thermal conductivity instrument, and the sample size was 30mm×1mm;
[0121] Flame retardant performance test: Use oxygen index tester to test the LOI of epoxy resin cured sample, the sample size is 130mm×6.5mm×3.2mm;
[0122] Room temperature and high temperature mechanical properties test: Taking AGB / T 3356 as the reference standard, a universal testing machine was used to conduct a three-point bending test on the cast glue cured sample at the experimental temperatures of 25°C and 100°C.
[0123]
[0124]
[0125] According to the data in the above table, we can clearly draw the following conclusions:
[0126] The epoxy resin cured product and the casting adhesive cured product obtained in Examples 1-3 are compared with the epoxy resin cured product and the casting adhesive cured product obtained in Comparative Examples 1-3. The test results show that:
[0127] Compared with the comparative example, the epoxy resin cured product obtained in Examples 1-3 has a higher oxygen index data, and the obtained casting adhesive cured product has higher room temperature and high temperature bending strength data and maintains good thermal conductivity. This fully demonstrates that the casting adhesive prepared by the present invention has excellent high temperature resistance, thermal conductivity and flame retardancy.
[0128] Compared with Example 1, the flame retardant epoxy resin in Comparative Example 1 is prepared from components such as melamine and trivinyltrimethylcyclotrisilazane; the flame retardant epoxy resin in Comparative Example 2 is prepared from components such as 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane and trivinyltrimethylcyclotrisilazane; the flame retardant epoxy resin in Comparative Example 3 is E-44. The epoxy resin system obtained in Comparative Examples 1-3 has a reduced oxygen index of the cured product; the obtained casting adhesive has a reduced crosslinking density of the cured product, and the room temperature and high temperature flexural strength and thermal conductivity data are reduced. It can be seen that the setting of the casting adhesive components and their processes of the present invention can promote the improvement of its high temperature resistance, thermal conductivity and flame retardancy.
[0129] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.
[0130] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive. Features: The process includes: mixing epoxy resin with flame retardant epoxy resin, plasticizer, thermal conductive filler and flame retardant filler in sequence, adding curing agent and accelerator, dispersing evenly, and obtaining casting glue; The flame retardant epoxy resin is prepared by the following process: S1. Mix dibenzaldehyde and anhydrous ethanol, heat to 50-60°C, stir and add melamine, heat to 85-90°C, continue stirring, and keep warm for reflux reaction for 8-10 hours to obtain an aldehyde compound; S2, mixing the aldehyde compound, diamine and anhydrous ethanol, heating to 60-75°C, stirring and reflux for 3-5h; adding DOPO, heating to 85-95°C, reacting for 16-18h to obtain an amino compound; S3, mixing the amino compound, alkenyl silane and anhydrous toluene, raising the temperature to 100-110° C., and reacting for 2-4 hours to obtain an alkenyl compound; S4, mixing the alkenyl compound and chloroform, adding glacial acetic acid and concentrated sulfuric acid, stirring and heating to 70-80° C., slowly adding hydrogen peroxide, and reflux reaction for 6-8 hours to obtain a flame retardant epoxy resin; The benzaldehyde is 4-(4-formylphenoxy)benzaldehyde, 2,2'-oxybenzaldehyde, 4,4'-diformyltriphenylamine, 2,7-benzaldehyde-benzothiadiazole, 9,10-di(4-formylphenyl)anthracene, 4,4'-(pyrene-1,6-diyl)benzaldehyde, 4,4'-(naphthalene-1,4-diyl)benzaldehyde, 4,4-(piperazine-1,4-diyl)benzaldehyde, 2,9-bis[ One of P-(formyl)phenyl]-1,10-phenanthroline, 4,4'-(1,10-phenanthroline-3,8-diyl)benzaldehyde, 4,4'-([2,2'-bipyridine]-5,5'-diyl)benzaldehyde, 4,4'-(1H-benzo[D]imidazole-4,7-diyl)benzaldehyde, and 4,4'-[biphenyl-4,4'-diylbis(1-naphthalen-1-ylazadiyl)]benzaldehyde; The alkenyl silane is one or a mixture of trivinyltrimethylcyclotrisilazane and 2,4,6-trivinyl-2,4,6-trimethylcyclotrisiloxane; The thermal conductive filler comprises boron nitride and aluminum oxide in a mass ratio of (1.7-3.0):1; The boron nitride is surface modified by the following process: Boron nitride, dopamine hydrochloride, Tris buffer and ethanol are mixed and ultrasonically dispersed for 20 to 30 minutes; stirred and reacted for 12 hours; the temperature is raised to 80 to 90°C, an amino compound is added, and stirred and reacted at a speed of 1000 to 1500 rpm for 6 to 8 hours to obtain modified boron nitride; The surface modification of the aluminum oxide is carried out as follows: Mix alumina and acetone, add KH-560, stir for 60-75 minutes, place at 60-65°C, continue stirring for 3-4 hours; cool, wash, and dry at 80-85°C to obtain modified alumina.
2. A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive according to claim 1, Features: The diamine is one of 1,3-bisaminopropyl-1,1,3,3-tetramethyldisiloxane, 1,2-diaminocyclohexane and 1,6-hexanediamine.
3. A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive according to claim 1, Features: The casting glue comprises the following components by mass: 60 to 80 parts of epoxy resin, 20 to 40 parts of flame-retardant epoxy resin, 10 to 30 parts of thermal conductive filler, 8 to 10 parts of flame-retardant filler, 6 to 10 parts of plasticizer, 74 to 85 parts of curing agent and 0.5 to 2.0 parts of accelerator.
4. A method for preparing a high temperature resistant and high thermal conductivity insulating casting adhesive according to claim 1, Features: The flame retardant filler is one of aluminum hydroxide and magnesium hydroxide or a mixture of the two.
5. Application of a high temperature resistant and high thermal conductivity insulating casting adhesive prepared by the preparation method according to any one of claims 1 to 4, Features: Used in the field of electronic packaging casting; the process is: inject casting glue into the area to be cast and solidify; The curing process conditions are: keeping warm at 60-80°C for 30 minutes; heating to 100-120°C and keeping warm for 2-3 hours; heating to 140-160°C and keeping warm for 2-3 hours; cooling to 120-140°C and keeping warm for 1-2 hours; cooling to 80-100°C and keeping warm for 1-2 hours.
Citation Information
Patent Citations
DOPO-based symtriazine ring hydrogenated benzimidazole epoxy curing agent and preparation method thereof
CN104086751A
Melamine-based nitrogen and phosphorus-containing compound, preparation method and application thereof, and flame-retardant epoxy resin composition of melamine-based nitrogen and phosphorus-containing compound
CN112679545A
Resin material and preparation method thereof
CN114426757A
Process for producing triepoxy ethyl cyclohexane and epoxy resin
JP2011195483A