A kind of ultra-low temperature resistant high-strength constant expansion alloy and preparation method thereof

By adding Mn, Ni, Co, Nb and other elements to the 4J29 alloy, and using vacuum smelting, vacuum self-consumption, forging and deep cold treatment, an ultra-low temperature resistant high-strength fixed expansion alloy was prepared, which solved the alloy at extremely low temperatures. The problems of unstable phase transition and insufficient strength achieve high strength and stable expansion performance at extremely low temperatures.

CN118389956BActive Publication Date: 2024-11-08XIAN GANGYAN SPECIAL ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410519061.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-28
Publication Date
2024-11-08
Estimated Expiration
2044-04-28

AI Technical Summary

Technical Problem

The existing 4J29 alloy may undergo martensite phase transition under extremely low temperature conditions, resulting in unpredictable expansion behavior and its strength is insufficient to meet high requirements such as aerospace.

Method used

A high-strength, ultra-low temperature resistant, high-strength fixed expansion alloy with components including Mn, Ni, Co, Nb and Fe, is prepared by vacuum smelting and vacuum self-consumption dual processes, combining forging, hot rolling and deep-cold treatment to ensure the alloy tissue uniformity and high strength.

Benefits of technology

The alloy has no martensite phase transition at -180°C, has a room temperature tensile strength of 750-850 MPa, and has a stable thermal expansion coefficient in the temperature range of 20-450°C, which significantly improves its ultra-low temperature and high strength properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389956B_ABST
    Figure CN118389956B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of precision alloy processing, and specifically relates to a ultra-low temperature resistant high-strength constant expansion alloy and a preparation method thereof, wherein the alloy comprises, by mass percentage: Mn: 0.30-0.50%, Ni: 29.0%-29.5%, Co: 17.0-17.5%, Nb: 0.2-0.4%, and the rest is Fe. The present invention uses fine steel as a vacuum smelting raw material for smelting, and adopts a vacuum smelting + vacuum consumable dual process, so that the ultra-low temperature resistance and high strength performance of the alloy are significantly improved; the alloy composition is regulated and the trace element Nb is added, and the Nb element can enhance fine grain strengthening, increase the strength of the alloy, stabilize the austenite phase, and make the alloy have no obvious martensitic phase transformation at 180°C, and has broad application potential in aerospace, electronics industry, energy and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of precision alloy processing, and in particular relates to an ultra-low temperature resistant high-strength constant expansion alloy and a preparation method thereof. Background Art

[0002] 4J29 alloy, known to the public as Kovar alloy, is an important material in the electronics industry. As a representative of Fe-Ni-Co hard glass sealing alloys, it plays an indispensable role in the glass sealing of electric vacuum components. Whether it is a transmitting tube, an oscillating tube or various other microelectronic devices, its stable performance and excellent low-temperature structural stability provide a solid guarantee for the reliability and durability of electronic products. However, each material has its limitations. Although the 4J29 alloy manufactured in accordance with the "YB / T5231-2014" standard has excellent performance in thermal expansion coefficient, its performance will change under extremely low temperature conditions. Especially below -78.5℃, the alloy may experience a martensitic phase transformation, causing its expansion behavior to become unpredictable. This phase transformation is undoubtedly a disaster for precision electronic sealing parts, which may cause the sealing parts to crack, thereby affecting the normal operation of the entire electronic equipment.

[0003] In addition, although 4J29 alloy has shown sufficient strength in general applications, its strength of about 450MPa is somewhat insufficient in fields such as aerospace, which have extremely high requirements for material performance. Aerospace equipment often needs to operate under ultra-low temperature, ultra-high pressure and extremely strong physical impact, which undoubtedly poses unprecedented challenges to the strength and stability of materials. Summary of the invention

[0004] 1. Purpose of the invention

[0005] The purpose of the present invention is to provide an ultra-low temperature resistant high-strength constant expansion alloy which can withstand ultra-low temperatures and improve its own strength, and a preparation method thereof.

[0006] (II) Technical solution

[0007] To solve the above problems, the present invention provides a ultra-low temperature resistant high-strength constant expansion alloy, which comprises, by mass percentage, Mn: 0.30-0.50%, Ni: 29.0-29.5%, Co: 17.0-17.5%, Nb: 0.2-0.4%, and the rest is Fe.

[0008] In another aspect of the present invention, preferably, the alloy further comprises, by mass percentage: C≤0.015%, P≤0.01%, S≤0.01%, Si≤0.30%, Cu≤0.10%, Cr≤0.10%, and Mo≤0.10%.

[0009] In another aspect of the present invention, preferably, the thermal expansion coefficient of the alloy in the temperature range of 20-400°C is (4.8-5.2)×10 -6 / ℃, the thermal expansion coefficient in the temperature range of 20-450℃ is (5.1-5.4)×10 -6 / ℃; the alloy has no martensitic phase transformation at -180℃, and the room temperature tensile strength of the alloy plate is 750-850MPa.

[0010] In another aspect of the present invention, preferably, a method for preparing an ultra-low temperature resistant high-strength constant expansion alloy is provided, wherein the method is used to prepare the ultra-low temperature resistant high-strength constant expansion alloy as described above, and the method comprises the following steps:

[0011] Step 100: weighing raw materials according to a preset raw material ratio, wherein the raw materials include Fe, Ni, Co, Nb and Mn;

[0012] Step 200: performing a first heat treatment on Fe, Ni, Co and Nb in the raw material to obtain a first alloy;

[0013] Step 300: adding Mn to the first alloy and performing a second hot working to obtain a second alloy;

[0014] Step 400: performing vacuum consumable remelting on the second alloy to obtain a third alloy;

[0015] Step 500: Forging the third alloy to obtain a fourth alloy;

[0016] Step 600: hot rolling the fourth alloy to obtain a fifth alloy;

[0017] Step 700: heat-treating the fifth alloy to obtain a high-strength constant expansion alloy resistant to ultra-low temperature.

[0018] In another aspect of the present invention, preferably, the step 200 of subjecting the Fe, Ni, Co and Nb in the raw material to a first hot working to obtain a first alloy comprises:

[0019] Step 201: baking the raw materials Fe, Ni, Co and Nb at a temperature of 400 to 600° C. for 5 to 6 hours;

[0020] Step 202: vacuum melting the baked raw material, wherein the vacuum melting includes a first time period and a second time period;

[0021] The vacuum degree in the first time period of the vacuum melting is less than or equal to 10Pa, the heating power in the first time period of the vacuum melting is 300-350kW, and the heating time is 30-35min.

[0022] Step 203: The vacuum degree in the second time period of the vacuum melting is less than or equal to 1 Pa, the heating power in the second time period is 500-550 kW, and after the temperature rises to the refining temperature, the refining temperature is maintained for 30-35 minutes, and timed deoxidation is performed to obtain the first alloy.

[0023] In another aspect of the present invention, preferably, the step 300 of adding Mn to the first alloy and performing a second hot working to obtain a second alloy comprises:

[0024] Step 301: adding Mn to the first alloy to perform a second hot working, wherein the heating power of the second hot working is 500-550 kW, and the stirring time of the second hot working is 1-2 min;

[0025] Step 302: Adjust the temperature to 1500-1530° C., cast the alloy ingot out of the furnace, air-cool for 3-5 hours, and then demould to obtain the second alloy.

[0026] In another aspect of the present invention, preferably, the step 400 of performing vacuum consumable remelting on the second alloy to obtain the third alloy comprises:

[0027] Step 401: removing the oxide scale of the second alloy and baking at a temperature of 800-850° C. for 8-9 hours;

[0028] Step 402: welding the baked second alloy to the dummy electrode, and performing vacuum consumable remelting, wherein the vacuum degree is less than or equal to 0.2 Pa, and the vacuum consumable remelting includes a first stage, a second stage, and a third stage, wherein the current of the first stage is 3000-4000A, the current of the second stage is 8000-9000A, and the current of the third stage is 4000A-4500A;

[0029] Step 403: After the vacuum consumable remelting is completed, the mold is demoulded after cooling for 3 to 5 hours, and then sand-cooled to obtain a third alloy.

[0030] In another aspect of the present invention, preferably, the step 500 of forging the third alloy to obtain the fourth alloy comprises: the forging comprises a first heating and a second heating;

[0031] Step 501: performing a first heating on the third alloy, wherein the first heating temperature is 800-900° C. and the first heating and heat preservation time is 50-70 min.

[0032] Step 502: performing a second heating on the third alloy that has completed the first heating, wherein the temperature of the second heating is 1100-1150° C., and the holding time of the second heating is 80-100 min;

[0033] Step 503: Forging the third alloy after the second heating;

[0034] Step 504: Forging to a slab size to obtain a fourth alloy; the forging includes three fires, each of which is cooled in air after forging, the deformation range of each fire is 50%-70%, and the final forging temperature is ≥850°C.

[0035] In another aspect of the present invention, preferably, the step 600 of hot rolling the fourth alloy to obtain the fifth alloy comprises:

[0036] Step 601: heating the fourth alloy at a temperature of 1050-1100° C. and a holding time of 25-35 min;

[0037] Step 602: hot rolling the heated fourth alloy;

[0038] Step 603: hot rolling to a hot-rolled size to obtain a fifth alloy; the hot rolling includes three passes, and the final rolling temperature is ≥800°C.

[0039] In another aspect of the present invention, preferably, the step 700 of heat treating the fifth alloy to obtain an ultra-low temperature resistant high strength constant expansion alloy comprises:

[0040] Step 701: placing the fifth alloy in liquid nitrogen for deep cooling, wherein the deep cooling time is 4 to 6 hours;

[0041] Step 702: taking the fifth alloy out of liquid nitrogen and performing aging treatment, heating to 550±10° C. at a rate of 5° C. / min, and keeping the temperature for 50 to 70 min;

[0042] Step 703: Temper the fifth alloy after aging treatment; cool down to 200-300° C. at a rate of 10° C. / min, and keep warm for 110-130 minutes to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

[0043] (III) Beneficial effects

[0044] The above technical solution of the present invention has the following beneficial technical effects:

[0045] The present invention uses refined steel as vacuum smelting raw material for smelting, and adopts vacuum smelting + vacuum consumable double process. The "vacuum + vacuum consumable" double process is adopted. Smelting in a vacuum environment can effectively avoid the reaction of gases such as oxygen and nitrogen in the atmosphere with the molten alloy, thereby reducing the gas content and non-metallic inclusions in the alloy, and the purity of the alloy is significantly improved; the vacuum consumable process can further remove impurities and gases in the alloy, because impurities and gases are more easily volatilized or removed during the melting process; through the combination of vacuum smelting and vacuum consumable double process, the alloy undergoes Multiple thermal cycles and composition homogenization processes help to eliminate coarse columnar crystals and segregation in the cast structure, making the alloy structure more uniform and fine; the uniform and fine grain structure and the reduction of gas in the alloy can significantly improve its ultra-low temperature resistance and the high strength performance of the alloy; forging is carried out in three passes, and each pass ensures a deformation of 50%-70%, which can break the structure of the alloy ingot; hot rolling is divided into three passes, using a small-large-small deformation composition, which can make the material structure fine and stable, and increase strength and phase change stability; deep cryogenic treatment + aging treatment + tempering treatment are combined to improve its phase change stability. The alloy composition is regulated and the trace element Nb is added. The Nb element can enhance the fine grain strengthening. During the solidification process of the alloy, the Nb element can serve as the core of heterogeneous nucleation, increase the nucleation rate, and thus refine the grains. At the same time, the Nb element can also hinder the growth of grains and further keep the grains small. The fine grains can increase the number of grain boundaries, which are obstacles to dislocation movement. Therefore, the strength of the alloy can be improved, the austenite phase can be stabilized, and the alloy can be free of martensitic phase transformation at -180°C. Since this alloy has good ultra-low temperature resistance and high strength characteristics, it has wide application potential in aerospace, electronics industry, energy and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 It is an overall preparation flow chart of an embodiment of the present invention. DETAILED DESCRIPTION

[0047] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0048] Obviously, the described embodiments are only some embodiments of the present invention, but not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] In the description of the present invention, it should be noted that the terms “first”, “second” and “third” are only used for descriptive purposes and cannot be understood as indicating or implying relative importance.

[0050] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0051] A super-low temperature resistant high-strength constant expansion alloy comprises, by mass percentage, 0.30-0.50% Mn, 29.0%-29.5% Ni, 17.0-17.5% Co, 0.2-0.4% Nb, and the rest Fe.

[0052] Furthermore, the alloy further comprises, by mass percentage: C≤0.015%, P≤0.01%, S≤0.01%, Si≤0.30%, Cu≤0.10%, Cr≤0.10%, and Mo≤0.10%.

[0053] Furthermore, the thermal expansion coefficient of the alloy within the temperature range of 20-400°C is (4.8-5.2)×10 -6 / ℃, the thermal expansion coefficient in the temperature range of 20-450℃ is (5.1-5.4)×10 -6 / ℃.

[0054] Furthermore, the alloy has no martensitic phase transformation at -180°C, and the room temperature tensile strength of the alloy plate is 750-850 MPa.

[0055] A method for preparing an ultra-low temperature resistant high-strength constant expansion alloy, the method being used to prepare the ultra-low temperature resistant high-strength constant expansion alloy as described above, Figure 1 FIG. 1 shows an overall flow chart of an embodiment of the present invention, as shown in FIG. Figure 1 As shown, the preparation method comprises the following steps:

[0056] Step 100: weighing raw materials according to a preset raw material ratio, wherein the raw materials include Fe, Ni, Co, Nb and Mn; wherein Mn: 0.30-0.50%, Ni: 29.0%-29.5%, Co: 17.0-17.5%, Nb: 0.2-0.4%, and the rest is Fe; wherein Ni purity is ≥99.99%; Co purity is ≥99.95%; Mn purity is ≥99.9%; Fe is fine steel pure iron, purity is ≥99.99%; high purity raw materials are conducive to controlling and significantly reducing the impurity content of the final alloy;

[0057] Step 200: performing a first heat treatment on Fe, Ni, Co and Nb in the raw material to obtain a first alloy, comprising:

[0058] Step 201: baking the raw materials Fe, Ni, Co, and Nb at a temperature of 400 to 600° C. for 5 to 6 hours; the purpose of baking is to dry the materials and remove moisture;

[0059] Step 202: vacuum melting the baked raw materials, wherein the vacuum melting includes a first time period and a second time period; the vacuum melting is heated by a medium frequency vacuum induction melting furnace; after baking, the raw materials are sequentially loaded into a crucible of the medium frequency vacuum induction melting furnace, wherein Ni is loaded at the bottom of the crucible, Fe is loaded around the crucible, and Co and Nb are loaded in the middle of the crucible. This loading method not only takes into account the physical and chemical properties of the raw materials, but also optimizes the heat distribution and the mixing effect of the alloy elements during the melting process;

[0060] The vacuum degree in the first time period of the vacuum melting is less than or equal to 10Pa, the heating power in the first time period of the vacuum melting is 300-350kW, and the heating time is 30-35min.

[0061] Step 203: the vacuum degree of the second time period of the vacuum melting is less than or equal to 1Pa, the heating power of the second time period is 500-550kW, after the temperature rises to the refining temperature, the refining temperature is maintained for 30-35min, and deoxidation is performed at regular intervals to obtain the first alloy; the refining temperature here is 1550℃-1580℃; during the refining period, a deoxidizer is added every 10 minutes, and the deoxidizer is aluminum powder;

[0062] The vacuum control in the first period helps to initially remove the air and impurity gases in the furnace to prevent the metal from being oxidized during the smelting process. Heating with a lower power can ensure that the metal material is heated evenly, laying a good foundation for the subsequent smelting process.

[0063] In the second period, the vacuum degree is further increased to less than or equal to 1Pa, and the heating power is increased to 500-550kW. Higher vacuum degree and heating power can promote rapid melting and uniform mixing of metal materials; help to remove gas and impurities in metal materials, thereby improving the purity of the alloy;

[0064] During refining, adding deoxidizers, such as aluminum powder, every 10 minutes can further remove oxides and other impurities in the alloy to ensure the high purity and uniformity of the alloy. At the same time, aluminum powder as a deoxidizer can also improve the fluidity and casting performance of the alloy;

[0065] Step 300: adding Mn to the first alloy and performing a second hot working to obtain a second alloy, comprising:

[0066] Step 301: adding Mn to the first alloy to perform a second hot working, wherein the heating power of the second hot working is 500-550 kW, and the stirring time of the second hot working is 1-2 min;

[0067] Step 302: adjusting the temperature to 1500-1530° C., casting the alloy ingot out of the furnace, air cooling for 3-5 hours and then demolding to obtain the second alloy;

[0068] The addition of Mn can significantly improve the mechanical properties of the alloy, such as tensile strength, yield strength and elastic modulus; Mn can refine the crystal structure in the alloy, thereby improving its mechanical properties; Mn can also improve the hardenability of the alloy, making it easier to perform hot working; the stirring operation during the second hot working process can ensure that the Mn element is evenly distributed in the alloy, thereby avoiding uneven performance or local weakening; stirring not only promotes the homogenization of the alloy composition, but also helps to eliminate internal pores and inclusions, further improving the quality of the alloy; pouring at a temperature range of 1500-1530℃ can ensure that the alloy has good fluidity, which is convenient for filling the mold and obtaining the ideal casting shape; demolding after air cooling for 3-5 hours helps the alloy to maintain sufficient strength while avoiding excessive internal stress and deformation;

[0069] Step 400: performing vacuum consumable remelting on the second alloy to obtain a third alloy comprises:

[0070] Step 401: removing the oxide scale of the second alloy and baking at a temperature of 800-850° C. for 8-9 hours;

[0071] Step 402: welding the baked second alloy to the dummy electrode, and performing vacuum consumable remelting, wherein the vacuum degree is less than or equal to 0.2 Pa, and the vacuum consumable remelting includes a first stage, a second stage, and a third stage, wherein the current of the first stage is 3000-4000A, the current of the second stage is 8000-9000A, and the current of the third stage is 4000A-4500A;

[0072] The first stage is 5 to 10 minutes, the second stage is before the weight of the unmelted alloy ingot accounts for about 15% of the total weight of the alloy ingot, and the third stage is after the weight of the unmelted alloy ingot accounts for about 15% of the total weight of the alloy ingot;

[0073] Step 403: After the vacuum consumable remelting is completed, the mold is removed after cooling for 3 to 5 hours, and then sand cooling is performed after demolding to obtain a third alloy;

[0074] The vacuum consumable process can further remove impurities and gases in the alloy, because impurities and gases are more likely to volatilize or be eliminated during the melting process; through the combination of vacuum melting and vacuum consumable double process, the alloy undergoes multiple thermal cycles and composition homogenization processes during melting and solidification, which helps to eliminate the coarse columnar crystals and segregation in the cast structure, making the alloy structure more uniform and fine; the uniform and fine grain structure and the reduction of gas in the alloy can significantly improve its ultra-low temperature resistance and the high strength performance of the alloy;

[0075] Step 500: Forging the third alloy to obtain a fourth alloy includes:

[0076] The forging includes a first heating and a second heating, using a high temperature resistance furnace for heating;

[0077] Step 501: performing a first heating on the third alloy, wherein the first heating temperature is 800-900° C. and the first heating and heat preservation time is 50-70 min.

[0078] Step 502: performing a second heating on the third alloy that has completed the first heating, wherein the temperature of the second heating is 1100-1150° C., and the holding time of the second heating is 80-100 min;

[0079] Step 503: Forging the third alloy after the second heating;

[0080] Step 504: Forging to the size of a flat billet to obtain a fourth alloy; the forging includes three fires, each of which is cooled in air after forging, the deformation range of each fire is 50%-70%, and the final forging temperature is ≥850°C; the first fire is to roughen the original specification of the third alloy φ420*1000 after the second heating to 500 high, the second fire is to change the direction and forge it into a square billet of 200*200*L, and the third fire is forged to 200*100*L;

[0081] Through the first heating and the second heating insulation process, the elements in the alloy have more time to diffuse, making the structure more uniform. The deformation during the forging process can break the coarse grains, further refine the alloy structure, and improve its mechanical properties and process performance; through precise forging steps, the matrix of the alloy is strengthened, the dislocation density is increased, and the strength and hardness of the alloy are improved. Forging is carried out in three fires, and each fire guarantees a deformation of 50%-70%, which can break the structure of the third alloy.

[0082] Step 600: hot rolling the fourth alloy to obtain a fifth alloy comprises:

[0083] Step 601: heating the fourth alloy at a temperature of 1050-1100° C. and a holding time of 25-35 min;

[0084] Step 602: hot rolling the heated fourth alloy;

[0085] Step 603: hot rolling to a hot rolling size to obtain a fifth alloy; the hot rolling includes three passes, and the final rolling temperature is ≥800° C.;

[0086] The rolling is completed in three passes. The first pass is from 100*200*L to 73*200*L. A small deformation is first performed, and the oxides on the surface of the billet are blown away. The second pass is rolled to 40*200*L. The large deformation in the middle refines the material grains. The deformation should be guaranteed to be 45%-55%. The third pass is rolled to 25*200*L. The small deformation releases the internal stress of the material at the same time. The hot rolling is divided into three passes, with a small-large-small deformation composition, which can make the material structure fine and stable, increase strength and phase change stability;

[0087] Step 700: heat treating the fifth alloy to obtain an ultra-low temperature resistant, high-strength, constant expansion alloy, including:

[0088] Step 701: placing the fifth alloy in liquid nitrogen for deep cooling, wherein the deep cooling time is 4 to 6 hours;

[0089] Step 702: taking the fifth alloy out of liquid nitrogen and performing aging treatment, heating to 550±10° C. at a rate of 5° C. / min, and keeping the temperature for 50 to 70 min;

[0090] Step 703: Temper the fifth alloy after aging treatment; cool down to 200-300° C. at a rate of 10° C. / min, and keep warm for 110-130 minutes to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

[0091] The combination of deep cryogenic treatment + aging treatment + tempering treatment improves its phase change stability.

[0092] Example 1

[0093] The raw materials are weighed according to the preset raw material ratio, and the raw materials include Fe, Ni, Co, Nb and Mn; Mn: 0.32%, Ni: 29.0%, Co: 17.2%, Nb: 0.20%, and the balance is Fe;

[0094] The raw materials Fe, Ni, Co and Nb are baked at a baking temperature of 400°C for 5 hours; a medium frequency vacuum induction melting furnace crucible is used for vacuum melting, Ni is loaded at the bottom of the crucible, Fe is loaded around the crucible, Co and Nb are loaded in the middle of the crucible, and the baked raw materials are vacuum melted, after the vacuum degree of the first time period of vacuum melting is 9Pa, the heating power of the first time period of vacuum melting is 300kW, the time of the first time period of vacuum melting is 30min, the vacuum degree of the second time period of vacuum melting is reduced to 0.5Pa, the heating power of the second time period of vacuum melting is 500kW, after the third heating temperature reaches the refining temperature, the refining temperature is maintained for 30min, and timed deoxidation is performed to obtain the first alloy, and the timed deoxidation method includes adding a deoxidizer every ten minutes for deoxidation; the deoxidizer is aluminum powder, and the refining temperature here is 1550°C;

[0095] Adding Mn to the first alloy for a second hot working, the heating power of the second hot working is 500 kW, and the stirring time of the second hot working is 1 minute; adjusting the temperature to 1500° C., pouring the alloy ingot out of the furnace, air cooling for 3 hours and then demolding to obtain the second alloy;

[0096] The oxide scale of the second alloy is removed, the second alloy is sawn at the head and tail, the surface is polished, the oxide scale is removed, and it is baked at a temperature of 800°C for 8 hours; the baked second alloy is welded with a dummy electrode and vacuum consumable remelting is performed, the vacuum degree is 0.1Pa, the first stage current is 3000A, the first stage time is 5min, the second stage current is 8000A, the second stage voltage is 30V, and the third stage current is 4000A; demolding is performed after cooling for 3 hours, and sand cooling is performed after demolding to obtain the third alloy.

[0097] The third alloy is heated by a high temperature resistance furnace, the first heating temperature is 800°C, the first heat holding time is 50min, the third alloy that has completed the first heating is heated for the second time, the second heating temperature is 1100°C, and the second heating holding time is 80min; the third alloy that has completed the second heating is forged to a flat billet size to obtain a fourth alloy, the forging includes three fires, each fire is cooled in air after forging, the deformation amount of each fire is 50%, and the final forging temperature is 850°C; the first fire is to roughen the original specification of the third alloy that has completed the second heating from φ420*1000 to 500 high, the second fire is to change the direction and forge it into a square billet of 200*200*L, and the third fire is forged to 200*100*L;

[0098] The fourth alloy was hot rolled by heating in a high temperature resistance furnace at a temperature of 1050°C, a holding time of 25 minutes, and a final rolling temperature of 800°C. The rolling was completed in three passes. The first pass was rolled from 100*200*L to 73*200*L, and the oxides on the surface of the billet were purged and removed. The second pass was rolled to 40*200*L with a deformation of 45%. The third pass was rolled to 25*200*L. The fifth alloy was obtained.

[0099] The fifth alloy is placed in liquid nitrogen for deep cooling for 4 hours;

[0100] After the fifth alloy is taken out from liquid nitrogen, it is subjected to aging treatment, heated to 550°C at a rate of 5°C / min, and kept at this temperature for 50 minutes; tempered; cooled to 200°C at a rate of 10°C / min, and kept at this temperature for 110 minutes, to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

[0101] Example 2

[0102] The raw materials are weighed according to the preset raw material ratio, and the raw materials include Fe, Ni, Co, Nb and Mn; Mn: 0.30%, Ni: 29.2%, Co: 17.5%, Nb: 0.30%, and the balance is Fe;

[0103] The raw materials Fe, Ni, Co and Nb are baked at a temperature of 600°C for 6 hours; a medium frequency vacuum induction melting furnace crucible is used for vacuum melting, Ni is loaded at the bottom of the crucible, Fe is loaded around the crucible, Co and Nb are loaded in the middle of the crucible, and the baked raw materials are vacuum melted, after the vacuum degree of the first time period of vacuum melting is 10Pa, the heating power of the first time period of vacuum melting is 350kW, the time of the first time period of vacuum melting is 35min, the vacuum degree of the second time period of vacuum melting is reduced to 1Pa, the heating power of the second time period of vacuum melting is 550kW, after the third heating temperature reaches the refining temperature, the refining temperature is maintained for 35min, and timed deoxidation is performed to obtain the first alloy, and the timed deoxidation method includes adding a deoxidizer every ten minutes for deoxidation; the deoxidizer is aluminum powder, and the refining temperature here is 1580°C;

[0104] Adding Mn to the first alloy for a second hot working, the heating power of the second hot working is 550kW, and the stirring time of the second hot working is 2 minutes; adjusting the temperature to 1530°C, pouring the alloy ingot out of the furnace, air cooling for 5 hours and then demolding to obtain the second alloy;

[0105] The oxide scale of the second alloy was removed, the second alloy was sawn from head to tail, the surface was polished, the oxide scale was removed, and it was baked at a temperature of 850°C for 9 hours; the baked second alloy was welded with a dummy electrode and vacuum consumable remelting was performed, the vacuum degree was 0.2Pa, the first stage current was 4000A, the first stage time was 10min, the second stage current was 9000A, the second stage voltage was 40V, and the third stage current was 4500A; after cooling for 5 hours, the mold was demolded, and sand cooling was performed after demolding to obtain the third alloy.

[0106] The third alloy is heated by a high temperature resistance furnace, the first heating temperature is 900°C, the first heating holding time is 70 minutes, the third alloy that has completed the first heating is heated for the second time, the second heating temperature is 1150°C, and the second heating holding time is 100 minutes; the third alloy that has completed the second heating is forged to a flat billet size to obtain a fourth alloy, the forging includes three fires, each fire is cooled in air after forging, the deformation range of each fire is 70%, and the final forging temperature is 880°C; the first fire is to roughen the original specification of the third alloy that has completed the second heating from φ420*1000 to 300 high, the second fire is to change the direction and forge it into a square billet 200*330*L, and the third fire is forged to 200*100*L;

[0107] The fourth alloy was hot rolled by heating in a high temperature resistance furnace at a temperature of 1100°C, a holding time of 35 minutes, and a final rolling temperature of 820°C. The rolling was completed in three passes, the first pass was rolled from 100*200*L to 70*200*L, and the oxide on the surface of the billet was purged and removed at the same time, the second pass was rolled to 35*200*L, the deformation was 55%, and the third pass was rolled to 25*200*L. The fifth alloy was obtained.

[0108] The fifth alloy was placed in liquid nitrogen for deep cooling for 6 hours;

[0109] After the fifth alloy is taken out from liquid nitrogen, it is subjected to aging treatment, heated to 560°C at a rate of 5°C / min, and kept at this temperature for 70 minutes; tempered; cooled to 300°C at a rate of 10°C / min, and kept at this temperature for 130 minutes, to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

[0110] Example 3

[0111] The raw materials are weighed according to the preset raw material ratio, and the raw materials include Fe, Ni, Co, Nb and Mn; Mn: 0.46%, Ni: 29.3%, Co: 17.0%, Nb: 0.40%, and the balance is Fe;

[0112] The raw materials Fe, Ni, Co and Nb are baked at a temperature of 500°C for 5.5 hours; a medium frequency vacuum induction melting furnace crucible is used for vacuum melting, Ni is loaded at the bottom of the crucible, Fe is loaded around the crucible, Co and Nb are loaded in the middle of the crucible, and the baked raw materials are vacuum melted, after the vacuum degree of the first time period of vacuum melting is 8Pa, the heating power of the first time period of vacuum melting is 330kW, the time of the first time period of vacuum melting is 33min, the vacuum degree of the second time period of vacuum melting is reduced to 0.8Pa, the heating power of the second time period of vacuum melting is 530kW, after the third heating temperature reaches the refining temperature, the refining temperature is maintained for 33min, and timed deoxidation is performed to obtain the first alloy, and the timed deoxidation method includes adding a deoxidizer every ten minutes for deoxidation; the deoxidizer is aluminum powder, and the refining temperature here is 1560°C;

[0113] Adding Mn to the first alloy for a second hot working, the heating power of the second hot working is 530 kW, and the stirring time of the second hot working is 1.5 min; adjusting the temperature to 1530° C., pouring the alloy ingot out of the furnace, air cooling for 3 hours and then demolding to obtain the second alloy;

[0114] The oxide scale of the second alloy was removed, the second alloy was sawn from head to tail, the surface was polished, the oxide scale was removed, and the alloy was baked at a temperature of 830°C for 8.5 hours; the baked second alloy was welded with a dummy electrode and vacuum consumable remelting was performed with a vacuum degree of 0.2Pa, a first-stage current of 3500A, a first-stage time of 5min, a second-stage current of 8500A, a second-stage voltage of 30V, and a third-stage current of 4300A; the alloy was demolded after cooling for 3 hours, and sand-cooled after demolding to obtain the third alloy.

[0115] The third alloy is heated by a high temperature resistance furnace, the first heating temperature is 850°C, the first heating holding time is 60min, the third alloy that has completed the first heating is heated by a second heating, the second heating temperature is 1130°C, and the second heating holding time is 90min; the third alloy that has completed the second heating is forged to a flat billet size to obtain a fourth alloy, the forging includes three fires, each fire is cooled in air after forging, the deformation range of each fire is 60%, and the final forging temperature is 850°C; the first fire is to roughen the original specification of the third alloy that has completed the second heating from φ420*1000 to 400 high, the second fire is to change the direction and forge it into a square billet of 200*250*L, and the third fire is forged to 200*100*L;

[0116] The fourth alloy was hot rolled by heating in a high temperature resistance furnace at a temperature of 1080°C, a holding time of 30 minutes, and a final rolling temperature of 830°C. The rolling was completed in three passes. The first pass was rolled from 100*200*L to 70*200*L, and the oxides on the surface of the billet were purged and removed. The second pass was rolled to 35*200*L with a deformation of 50%. The third pass was rolled to 25*200*L. The fifth alloy was obtained.

[0117] The fifth alloy is placed in liquid nitrogen for deep cooling for 5 hours;

[0118] After the fifth alloy is taken out from liquid nitrogen, it is subjected to aging treatment, heated to 540°C at a rate of 5°C / min, and kept at this temperature for 60 minutes; tempered; cooled to 250°C at a rate of 10°C / min, and kept at this temperature for 120 minutes, to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

[0119] Example 4

[0120] The raw materials are weighed according to the preset raw material ratio, and the raw materials include Fe, Ni, Co, Nb and Mn; Mn: 0.50%, Ni: 29.5%, Co: 17.0%, Nb: 0.35%, and the balance is Fe;

[0121] The raw materials Fe, Ni, Co and Nb are baked at a baking temperature of 430°C for 5.2 hours; a medium frequency vacuum induction melting furnace crucible is used for vacuum melting, and the baked raw materials are vacuum melted, after the vacuum degree of the first time period of vacuum melting is 10Pa, the heating power of the first time period of vacuum melting is 320kW, the time of the first time period of vacuum melting is 32min, the vacuum degree of the second time period of vacuum melting is reduced to 1Pa, the heating power of the second time period of vacuum melting is 520kW, after the third heating temperature reaches the refining temperature, the refining temperature is maintained for 32min, and timed deoxidation is performed to obtain the first alloy, and the timed deoxidation method includes adding a deoxidizer every ten minutes for deoxidation; the deoxidizer is aluminum powder, and the refining temperature here is 1550°C;

[0122] Add Mn to the first alloy for a second hot working, the heating power of the second hot working is 520 kW, and the stirring time of the second hot working is 1 min; adjust the temperature to 1520° C., cast the alloy ingot out of the furnace, air cool for 3 hours, and then demould to obtain the second alloy;

[0123] The oxide scale of the second alloy was removed, the second alloy was sawn from head to tail, the surface was polished, the oxide scale was removed, and it was baked at a temperature of 820°C for 8.5 hours; the baked second alloy was welded with a dummy electrode and vacuum consumable remelting was performed, the vacuum degree was 0.1Pa, the first stage current was 3200A, the first stage time was 5min, the second stage current was 8200A, the second stage voltage was 30V, and the third stage current was 4200A; after cooling for 3 hours, the mold was demolded, and sand cooling was performed after demolding to obtain the third alloy.

[0124] The third alloy is heated by a high temperature resistance furnace, the first heating temperature is 820°C, the first heating holding time is 55min, the third alloy that has completed the first heating is heated by a second heating, the second heating temperature is 1100°C, and the second heating holding time is 80min; the third alloy that has completed the second heating is forged to a flat billet size to obtain a fourth alloy, the forging includes three fires, each fire is cooled in air after forging, the deformation range of each fire is 50%, and the final forging temperature is 850°C; the first fire is to roughen the original specification of the third alloy that has completed the second heating from φ420*1000 to 500 high, the second fire is to change the direction and forge it into a square billet of 200*200*L, and the third fire is forged to 200*100*L;

[0125] The fourth alloy was hot rolled by heating in a high temperature resistance furnace at a temperature of 1050°C, a holding time of 25 minutes, and a final rolling temperature of 800°C. The rolling was completed in three passes. The first pass was rolled from 100*200*L to 70*200*L, and the oxides on the surface of the billet were purged and removed. The second pass was rolled to 35*200*L with a deformation of 50%. The third pass was rolled to 25*200*L. The fifth alloy was obtained.

[0126] The fifth alloy was placed in liquid nitrogen for deep cooling for 4.5 hours;

[0127] After the fifth alloy is taken out from liquid nitrogen, it is subjected to aging treatment, heated to 545°C at a rate of 5°C / min, and kept at this temperature for 55 minutes; tempered; cooled to 280°C at a rate of 10°C / min, and kept at this temperature for 110 minutes, to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

[0128] Comparative Example 1

[0129] No Nb was added, vacuum melting was adopted, vacuum consumable remelting was not adopted, and the remaining operations were the same as those in Example 1;

[0130] Comparative Example 2

[0131] No Nb was added, and the remaining operations were the same as in Example 1.

[0132] Comparative Example 3

[0133] The raw materials are the same as those in Example 1, the steps are not cryogenically treated, and the remaining operations are the same as those in Example 1.

[0134] Comparative Example 4

[0135] The raw materials are the same as those in Example 1. The forging process in the steps includes two-time forging according to the "small + large" deformation law to the forging blank specifications, and the remaining operations are the same as those in Example 1.

[0136] Comparative Example 5

[0137] The raw materials are the same as those in Example 1. The hot rolling process in the steps includes two hot rollings according to the "small + large deformation rule" to the final specifications, and the remaining operations are the same as those in Example 1.

[0138] The element ratios of Examples 1-4 and Comparative Examples 1-2 are shown in Table 1, and the performance strengths of Examples 1-4 and Comparative Examples 1-2 are shown in Table 2.

[0139] Table 1 Element ratios of Examples 1-4 and Comparative Examples 1-5

[0140]

[0141] Table 2 Performance strength of Examples 1-4 and Comparative Examples 1-5

[0142]

[0143] The thermal expansion coefficient of the alloy in this embodiment within the temperature range of 20-400°C is (4.8-5.2)×10 -6 / ℃, the thermal expansion coefficient in the temperature range of 20-450℃ is (5.1-5.4)×10 -6 / ℃. The ultra-low temperature resistance and high strength performance of the alloy in this embodiment are significantly improved; the alloy has no martensitic phase transformation at -180℃. The strength of the alloys in Comparative Examples 1-5 is lower than that in Example 1, and Comparative Examples 3-5 have martensitic phase transformation at -180℃, indicating that the combined treatment of forging, hot rolling and deep cryogenic treatment + aging treatment + tempering treatment in the present invention can increase strength and phase transformation stability.

[0144] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

[0145] The present invention has been described above with reference to the embodiments of the present invention. However, these embodiments are for illustrative purposes only and are not intended to limit the scope of the present invention. The scope of the present invention is defined by the appended claims and their equivalents. Without departing from the scope of the present invention, a person skilled in the art may make various substitutions and modifications, which should all fall within the scope of the present invention.

[0146] Although the embodiments of the present invention have been described in detail, it should be understood that the various changes, substitutions, and alterations could be made hereto without departing from the spirit and scope of the invention.

[0147] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a super low temperature resistant high strength constant expansion alloy, characterized in that: The alloy comprises, by mass percentage, 0.30-0.50% Mn, 29.0-29.5% Ni, 17.0-17.5% Co, 0.2-0.4% Nb, and the remainder Fe; The preparation method comprises the following steps: Step 100: weighing raw materials according to a preset raw material ratio, wherein the raw materials include Fe, Ni, Co, Nb and Mn; Step 200: performing a first heat treatment on Fe, Ni, Co and Nb in the raw material to obtain a first alloy; Step 300: adding Mn to the first alloy and performing a second hot working to obtain a second alloy; Step 400: performing vacuum consumable remelting on the second alloy to obtain a third alloy; Step 500: Forging the third alloy to obtain a fourth alloy; Step 600: hot rolling the fourth alloy to obtain a fifth alloy; Step 700: heat-treating the fifth alloy to obtain a high-strength constant expansion alloy resistant to ultra-low temperature; The step 200 of subjecting Fe, Ni, Co and Nb in the raw material to a first heat treatment to obtain a first alloy comprises: Step 201: baking the raw materials Fe, Ni, Co and Nb at a temperature of 400 to 600° C. for 5 to 6 hours; Step 202: vacuum melting the baked raw material, wherein the vacuum melting includes a first time period and a second time period; The vacuum degree in the first time period of the vacuum melting is less than or equal to 10Pa, the heating power in the first time period of the vacuum melting is 300-350kW, and the heating time is 30-35min. Step 203: the vacuum degree in the second time period of the vacuum melting is less than or equal to 1 Pa, the heating power in the second time period is 500-550 kW, after the temperature rises to the refining temperature, the refining temperature is maintained for 30-35 minutes, and deoxidation is performed at a fixed time to obtain a first alloy; When charging, Ni is placed at the bottom of the crucible, Fe is placed around the crucible, and Co and Nb are placed in the middle of the crucible; during refining, a deoxidizer is added every 10 minutes, and the deoxidizer is aluminum powder; The step 300 of adding Mn to the first alloy and performing a second hot working to obtain a second alloy comprises: Step 301: adding Mn to the first alloy to perform a second hot working, wherein the heating power of the second hot working is 500-550 kW, and the stirring time of the second hot working is 1-2 min; Step 302: adjusting the temperature to 1500-1530° C., casting the alloy ingot out of the furnace, air cooling for 3-5 hours and then demolding to obtain the second alloy; The step 700: heat treating the fifth alloy to obtain an ultra-low temperature resistant, high-strength, constant expansion alloy comprises: Step 701: placing the fifth alloy in liquid nitrogen for deep cooling, wherein the deep cooling time is 4 to 6 hours; Step 702: taking the fifth alloy out of liquid nitrogen and performing aging treatment, heating to 550±10° C. at a rate of 5° C. / min, and keeping the temperature for 50 to 70 min; Step 703: Temper the fifth alloy after aging treatment; cool down to 200-300° C. at a rate of 10° C. / min, and keep warm for 110-130 minutes to obtain an ultra-low temperature resistant high-strength constant expansion alloy.

2. The preparation method according to claim 1, characterized in that: The alloy further comprises, by mass percentage: C≤0.015%, P≤0.01%, S≤0.01%, Si≤0.30%, Cu≤0.10%, Cr≤0.10%, and Mo≤0.10%.

3. The preparation method according to claim 1, characterized in that: The thermal expansion coefficient of the alloy in the temperature range of 20-400°C is (4.8-5.2)×10 -6 / ℃, the thermal expansion coefficient in the temperature range of 20-450℃ is (5.1-5.4)×10 -6 / ℃; the alloy has no martensitic phase transformation at -180℃, and the room temperature tensile strength of the alloy plate is 750-850MPa.

4. The preparation method according to claim 1, characterized in that: The step 400 of performing vacuum consumable remelting on the second alloy to obtain a third alloy comprises: Step 401: removing the oxide scale of the second alloy and baking at a temperature of 800-850° C. for 8-9 hours; Step 402: welding the baked second alloy to the dummy electrode, and performing vacuum consumable remelting, wherein the vacuum degree is less than or equal to 0.2 Pa, and the vacuum consumable remelting includes a first stage, a second stage, and a third stage, wherein the current of the first stage is 3000-4000A, the current of the second stage is 8000-9000A, and the current of the third stage is 4000A-4500A; Step 403: After the vacuum consumable remelting is completed, the mold is demoulded after cooling for 3 to 5 hours, and then sand-cooled to obtain a third alloy.

5. The preparation method according to claim 1, characterized in that: The step 500 of forging the third alloy to obtain the fourth alloy includes: the forging includes a first heating and a second heating; Step 501: performing a first heating on the third alloy, wherein the first heating temperature is 800-900° C. and the first heating and heat preservation time is 50-70 min. Step 502: performing a second heating on the third alloy that has completed the first heating, wherein the temperature of the second heating is 1100-1150° C., and the holding time of the second heating is 80-100 min; Step 503: Forging the third alloy after the second heating; Step 504: Forging to the size of a flat billet to obtain a fourth alloy; the forging includes three fires, each of which is cooled in air after forging, the deformation range of each fire is 50%-70%, and the final forging temperature is ≥850°C.

6. The preparation method according to claim 1, characterized in that: The step 600 of hot rolling the fourth alloy to obtain a fifth alloy comprises: Step 601: heating the fourth alloy at a temperature of 1050-1100° C. and a holding time of 25-35 min; Step 602: hot rolling the heated fourth alloy; Step 603: hot rolling to a hot-rolled size to obtain a fifth alloy; the hot rolling includes three passes, and the final rolling temperature is ≥800°C.